An Introduction to Slip Casting Ceramics with Multi-Piece Molds

Posted By Linda Gates On December 29, 2014 @ 5:07 am In Daily,Features,Making Ceramic Molds | 23 Comments

gates_620newPotter Linda Gates decorates her ceramic surfaces using commercial digital decals with imagery of everyday objects from the 1950s, including the paper dolls of that era. It was a project she started during her studies in the ceramic design program at Bath Spa University in England. Gates prefers to slip cast her forms so that the surfaces are as smooth as possible for the decal application.

 

Today, Gates walks us through the slip-casting process for one of her jug forms using a four-piece plaster mold for the body and a two-piece plaster mold for the handle. – Jennifer Harnetty, editor.

 


 

figure 1 – click to enlarge!

Ceramic decals can be applied to any glazed object, but it makes life easier if the ceramic form has smooth surfaces to avoid the problem of trapped air creating bubbles and holes in the image. The ceramic form shown here is a slip-cast jug that I designed as part of a college tableware design project.

 

With a little modification to the original jug design, I made new plaster molds, one for the handle (figure 1) and the other for the body of the form. The mold for the body of the jug (figure 2) is made in four parts – the two sides, the base, and the reservoir.

 

figure 2 – click to enlarge!

To prevent leaks when pouring the casting slip, secure the parts firmly together with strong bands cut from rubber inner tubes (figure 3). If you design your mold to include a reservoir, which makes it easier to maintain an even rim thickness, fill the mold to halfway up the reservoir wall using commercial earthenware casting slip. As the porous mold absorbs the water from the clay, the excess is drawn from the reservoir.

 

figure 3 – click to enlarge!

The handle mold is also filled with casting slip. Once the slip is the desired thickness (check by blowing on the edge of the mold where the slip and plaster meet), pour the extra casting slip back into the container and leave the mold inverted at an angle to drain into a bucket. Placing it at an angle avoids stalactites of clay forming on the bottom of the piece.

 

Tip: To achieve even thickness between multiple casts, it is a good idea to time the first casting and use this as a guideline.

 

figure 4 – click to enlarge!

When the mold is well drained and the sheen has gone from the wet casting slip (typically about 20 minutes), remove only the reservoir portion from the jug mold, trim the excess clay from the top and clean it up with a damp sponge. I leave the rest of the mold intact for a further hour or so for the form to firm up for easier handling.

 

figure 5 – click to enlarge!

Both molds are then disassembled and the jug form and handle carefully removed. Both component parts are cleaned up with a fettling knife and damp sponge. The handle is attached, and the form is covered in plastic for 24 hours to ensure a secure join.

 

To learn more about Linda Gates or see more images of her work, please visit http://www.lindagates.net/.

 

 


 

For great mold making techniques, be sure to download your free copy of Ceramic Mold Making Techniques: Tips for Making Plaster Molds and Slip Casting Clay, Volume II.

 


 


Article printed from Ceramic Arts Daily: http://ceramicartsdaily.org

URL to article: http://ceramicartsdaily.org/pottery-making-techniques/making-ceramic-molds/an-introduction-to-slip-casting-ceramics-with-multi-piece-molds/

Copyright © 2008-2012 Ceramic Arts Daily. All rights reserved.