Though gas kilns are not as ubiquitous as electric kilns these days, there  are still many potters and ceramic artists who rely on them to create the wonderful effects created in a reduction, salt, or soda atmosphere.

 

Most anyone can figure out how to mix gas and air to produce heat in a kiln. What takes a little more expertise is firing a kiln with efficiency, regardless of what type of firing is being done. In today’s post, Hal Frenzel explains how understanding fuel combustion will help you make the most of your gas kiln.- Jennifer Harnetty, editor.


What is perfect combustion? By reading the description in the North American Combustion Handbook, it seems rather simple: Perfect combustion exists when one carbon atom is combined with two atoms of oxygen to form one carbon dioxide molecule, plus heat. But when you are firing a kiln to achieve a certain consistent atmosphere, it becomes a little more complicated.

 

To achieve complete combustion, the exact proportions of fuel and oxygen are required with nothing remaining. In a gas kiln firing this is often difficult to attain because of the many variables in fuel and oxygen (which is derived from the air) and the equipment used to mix the two.

 

Get to know your kiln better with The Kiln Book!

 


 

The most common fuels used today are natural gas and propane. These are hydrocarbons and when they are properly mixed and ignited, they produce heat, carbon dioxide and water vapor.

 

Air is a combination of approximately 75% nitrogen and 25% oxygen by weight. Unlike oxygen, the nitrogen does not react (combust) but it still absorbs a portion of the heat and therefore creates a cooler flame.

 

When excess oxygen is present in the kiln, it plays no part in combustion. However, it does absorb heat energy that would otherwise help fire your ware. In this way, it does contribute to fuel consumption. (relieved of their oxygen molecules) by oxygen-hungry fuel. This typically results in a color change.

During the firing of a gas kiln there are a trio of atmospheres that have to be controlled to achieve both a rise in temperature and the desired glaze results. The first, and most important, atmosphere is neutral. It is only in a neutral atmosphere that perfect combustion can be attained. A neutral atmosphere is the most fuel-efficient firing possible.

 

If the amount of air is increased, or the amount of fuel is decreased, from a neutral firing, the mixture becomes fuel-lean and the flame is shorter and clearer. The kiln has now entered an oxidizing atmosphere and the rate of temperature rise will decrease.

 

If the fuel supply is increased or the air supply is decreased the atmosphere becomes fuel-rich and reduction begins. The flame becomes long and smoky and incomplete combustion occurs. The result is an excess of carbon, which combines with the remaining oxygen and creates carbon monoxide. To convert back to its natural state of carbon dioxide, the carbon takes oxygen from the metal oxides in the glaze, thus altering the finished color of the glaze. The rate of temperature rise will also diminish under these conditions.

 

Regardless of the atmosphere necessary for the results you desire for your work, a higher level of efficiency and fuel savings may be attained by firing to a neutral atmosphere whenever possible (see diagrams on page 38). With the enormous increases we have seen and will continue to see in fuel costs, it might become highly desirable to buy an oxygen probe and maintain a neutral atmosphere for at least part of your firings.

 

In the early stages of a firing, excess oxygen helps in the decomposition of the organic and inorganic carbonates and sulfates. In researching this article, I was unable to find a potter/ceramist who could explain exactly how excess oxygen during the glaze maturity period enhances the glaze finish or color. This raises the question as to whether the results would have been the same if fired in a neutral atmosphere during this period. If, by chance, the results are the same, then an oxidation potter would save both time and fuel if he or she fired in perfect combustion during this period.

 

Oxygen to burn fuel in an artist’s kiln comes from the air. The air, however, is not all oxygen. Rather, it is far from it. By weight, air is approximately 77% nitrogen and 23% oxygen. What this means to the artist is that for every ONE pound of oxygen from air that is heated to kiln temperature to burn fuel in a kiln, THREE pounds of nitrogen have to be heated to kiln temperature. This is why using “excess” oxygen is expensive. Using a minimum amount of excess air in an oxidation firing saves both energy and money.

 When an excess of carbon (fuel) or a shortage of oxygen (air) is introduced, incomplete combustion takes place. Carbon monoxide (as opposed to carbon dioxide) is produced along with heat, though not as much as would be produced during complete combustion. The carbon monoxide then looks for more oxygen, which it takes from oxides in the clay and glaze in the kiln. This is also the reason yellow flames shoot out through spy holes when a kiln is in reduction—the carbon-rich fuel is following the oxygen supply.

When an excess of carbon (fuel) or a shortage of oxygen (air) is introduced, incomplete combustion takes place. Carbon monoxide (as opposed to carbon dioxide) is produced along with heat, though not as much as would be produced during complete combustion. The carbon monoxide then looks for more oxygen, which it takes from oxides in the clay and glaze in the kiln. This is also the reason yellow flames shoot out through spy holes when a kiln is in reduction—the carbon-rich fuel is following the oxygen supply.

 

Defining the Terms

Oxidation Atmosphere: A mixture of fuel and air where there is a significant excess of oxygen from the air relative to the fuel; defined (somewhat arbitrarily) as more than 3% excess oxygen.

Neutral Atmosphere: A theoretical mixture of fuel and air where there is a perfect balance between the amount of fuel and the amount of oxygen from air necessary to burn that fuel.

Reduction Atmosphere: A mixture of fuel and air where there is more fuel present than there is oxygen from the air to burn the fuel. For complete combustion to occur in a reducing atmosphere, the fuel must react with all the oxygen from the incoming air and with oxygen from other sources. For a ceramics artist, the important “other” sources of oxygen are oxides of iron and/or copper in the ware being fired, as those oxides are reduced.

 

To learn more about kilns and help figure out which one is right for you, download your free copy of A Guide to Ceramic Kilns: Choosing the Right Kiln Firing Method and Design For Your Art.
 

Thinking about building or purchasing a kiln?

Then turn to the ultimate guide to designing, building, and firing ceramic kilns: The Kiln Book.

This trusted resource from Fred Olsen will help you understand what it takes to successfully harness the heat you need to fire your work and get the effects you’re looking for.

 

 

 