Building the Kiln
We began by laying out a 15-inch high foundation of concrete blocks, on which we placed 9 inches of K23 hard brick in an alternating header and stretcher fashion to create a total interior floor plan that measured 45×96 inches (figure 1). The first three feet of the interior was reserved for the firebox with the remaining five feet, tiered up 6 inches, for the ceramic ware. The flooring in the firebox area was constructed with K26 hard brick to better withstand the cone 10 temperatures we would be reaching. Similarly, the walls were constructed 9 inches thick by alternating courses of stretchers and headers to a height of 15 inches.
|
|
|
Download a printer-friendly version of this assignment here: |
|
|
Before adding the arch, we lined the outer walls of the kiln with cinder blocks to a height of 37 inches, then filled the blocks with rebar and mortar mix. The small 4-inch gap between the concrete blocks and the hard brick was then filled with pea gravel to support the force of the dome on the kiln wall and to increase insulation and to allow for thermal expansion (figure 2). The exit flue to the chimney was created slightly oversized at a total of 22½×22½ inches with the chimney interior at 13½×13½ inches. The chimney was built with hard brick to a height of 15 feet and finished with a 4-foot stack anchored with cables into the ground on three sides. A removable spanner brick was placed above the damper to act as a passive damper.
|
|
|
The Roof
Instead of making a wooden frame for the arched roof, we used excess dirt from the construction site of a nearby middle school to make a solid mound inside the kiln. With a couple shovels and a lot of muscle we piled on two truckloads of dirt to form a smooth curved dome. Once shaped to our liking, we then mixed high refractory castable to form the dome. Since we were on a budget, we mixed all 2400 pounds of castable by hand with a hoe and mortar tray to a consistency of thick concrete. Next, we lined the dirt with plastic bags and added one ball right on top of the other until the entire dome was completed to a thickness of 9 inches (figure 3). Using two plastic buckets, we added the balls around the buckets so that when the buckets were removed, we had negative spaces for side stoking (figure 4). After the last ball, we covered the entire dome with plastic bags to let it cure overnight. The next day we lined the dome with fiber blanket and an adobe mix of mortar, dirt and straw. This not only further insulated the kiln, but also protected the castable from the snow and rain.
|
|
|
Caution: As a safety precaution, everyone wore face masks and rubber gloves while handling the fiber blanket, as the small particles can irritate the lungs and the skin. Rubber gloves are recommended when handling adobe as wee. Concrete can irritate skin (and it makes your fingers pruney). After the castable set up, the door was disassembled and the dirt was removed. At last, after five days, the Lewis Central Anagama was complete.
Making Work
The next week was spent making a wide variety of pottery for the kiln. I provided three different clays to use with maturing rates from cone 6 to cone 10. In addition, a variety of tried-and-true high-fire glazes were supplied from copper reds to celadons and shinos. Students were encouraged to keep good notes of which clays and glazes were used for each piece to reflect on successes and learning experiences.
|
|
|
Getting Ready
Over the weekend, we spent one full day loading the pieces into the kiln. Tumble stacked one on top of the other, nearly every nook and cranny of the kiln was used. By Sunday, the front of the kiln was bricked up, leaving a main stoke hole and primary air inlets at the bottom of the door. Using a homemade block of castable, a U-bolt, an eyebolt and some chain, we were able to suspend a movable door from a post and lintel so that wood could be stoked with minimal heat loss. The post and lintel were made by setting two 8-foot 4×4 posts with a 10-foot 4×4 post for the horizontal beam and securing them with metal brackets. With the door in place and the kiln full of work, we were ready to go.
|
|
|
Firing
The kiln was started with a small fire at 5 PM on Sunday. By early Monday morning the kiln was nearing 1800ºF. Working in teams of two or three and stoking several split logs at the end of every reduction cycle, the kiln climbed to 2200ºF by Monday evening. We were at cone 10 by noon on Tuesday (figure 5) and held it at that temperature until 5 PM when we stopped stoking and sealed the kiln. To help ensure a slow cooling, we dipped newspapers into a large barrel of slip and completely coated the entire kiln with the dripping wet sheets to decrease heat loss. This, as you can imagine, was a fun and messy highlight of the entire experience.
|
|
|
The Results
After three days of cooling, it was time to open the kiln. The old adage of a unloading a kiln unloading feeling like Christmas morning could not be more apropos (figure 6). All of the students, young and old, came early to see their approximately 400 newly finished creations and enjoy a potluck meal with a new family of bonded potters. We had much to celebrate. We were able to load and fire the kiln in the course of a weekend with just under two cords of wood. We proved that an anagama is not only doable at the high school level, but an amazing learning tool that will provide students with a life-long experience. We will be firing it up again this summer and our pottery club is in full swing to fill the quota.
|
|
|
Clay Cunningham is a ceramic artist and instructor, currently teaching at Lewis Central High School in Council Bluffs, Iowa. To see more of his work, or for contact information, visit www.claycunningham.org.
|
|