Hi I am looking for a way to make my raw majolica glaze "harder" so that I can ddo more painterly desings on my ware. Mybrush tends to clog up with the glaze powder and so the lines are interrupted.
Hope somepone can help. I think I readd somewhere that you can spray something onto the glaze.Does any one have any hints.
Babs
Page 1 of 1
preparing raw majolica glaze for surface decoration.
#2
Posted 25 January 2013 - 10:31 PM
Here is a link to a handout from Linda Arbuckle on majolica, including hardening the base glaze . . . http://lindaarbuckle...handout2007.pdf
#9
Posted 07 February 2013 - 12:52 PM
add CMC to your base glaze. commercial glazes contain a good amount of this in their recipe. it forms sort of a "candy coating" and stiffens up the unfired glaze, which will be more resistant to your detail brush. start with around 1% or keep a thick solution of it in a jug to add to your glazes, underglazes, and stains/washes.