: shino -

Jump to content

Share Topic:   facebook stumbleupon del-icio-us digg email google mixx reddit
Page 1 of 1
  • You cannot start a new topic
  • You cannot reply to this topic

shino

#1 User is offline   Iforgot Icon

  • Advanced Member
  • PipPipPip
  • View gallery
  • Group: Members
  • Posts: 137
  • Joined: 20-May 12
  • LocationColorado

Posted 19 January 2013 - 09:39 PM

Hey world

I need a cone 5 oxidation shino recipie, any ieas? Thanks!


Darrel
Derek VonDrehle

Raku, Pit fired, Majolica, and Stoneware ceramic artisit
0

#2 User is offline   OffCenter Icon

  • Advanced Member
  • PipPipPip
  • View gallery
  • Group: Members
  • Posts: 975
  • Joined: 01-April 10
  • LocationLizella, Georgia

Posted 19 January 2013 - 10:24 PM

Oxidation Shino ^6
Alberta Slip ... 56.0
Gerstley Borate ... 18.7
Soda Feldspar ... 9.4
Silica ... 9.4
Lithium Carbonate ... 6.5
Zircopax ... 9.4
Tin Oxide ... 4.7

This one's pretty good. Fat and creamy where thick, orange where thin.

Jim
E pur si muove.

"But it does move," said Galileo under his breath.