Posted 09 January 2013 - 01:03 PM

I am a potter of some years and have been working with a Grolleg cone 6 body for the last year or so. I am continually frustrated by bloating. The bisque has been totally fine tuned. The problem is with larger pieces - thrown from 8 to 14 lbs. Is this air trapped in the walls? out gasing? I am firing the schedule from the Cone 6 Glaze guys . . . I am making extra everything for orders to cover the losses. HELP!!
0

#2 User is offline   neilestrick Icon

  • Neil Estrick
  • PipPipPip
  • Group: Members
  • Posts: 1,206
  • Joined: 04-October 11
  • LocationGrayslake, IL

Posted 09 January 2013 - 05:36 PM

If it's truly bloating, you'll generally get a lot of little bubbles. If you're getting just a couple of larger bubbles, then it's probably air bubbles. They tend to show up in porcelain. If it's bloating, you might try a different firing schedule or check the calibration of your kiln.
Neil Estrick
Kiln Repair Tech
L&L Distributor
Owner, Neil Estrick Gallery, LLC
www.neilestrickgallery.com

neil@neilestrickgallery.com
0

#3 User is offline   OffCenter Icon

  • Advanced Member
  • PipPipPip
  • View gallery
  • Group: Members
  • Posts: 986
  • Joined: 01-April 10
  • LocationLizella, Georgia

Posted 09 January 2013 - 07:07 PM

I don't think air bubbles cause bloating but they can look like bloating but those that look like bloating are already there before the pot is fired, just maybe not as noticeable. Bloated is often caused by over firing. For some clays even a slight over firing will cause bloating. If you're mixing up the clay, be sure it is well mixed because if it is not that can cause bloating. Organic matter can cause bloating but that's probably not a problem with porcelain. Carbon trapped in the clay can cause it and that's not only a problem in reduction (which I guess you're not doing) but in electric kilns with thick pieces tightly packed.

Wedge the clay more to make sure it is well-mixed. Test to see if you're over firing. If that doesn't solve the problem then try not packing the kiln as tight as usual and slow down around 700 degrees to let carbon escape. If that doesn't work, you need a new porcelain.

Jim
E pur si muove.

"But it does move," said Galileo under his breath.
0

#4 User is offline   Natania Hume Icon

  • Advanced Member
  • PipPipPip
  • Group: Members
  • Posts: 113
  • Joined: 10-July 11

Posted 09 January 2013 - 07:56 PM

View Postpam sinclair, on 09 January 2013 - 01:03 PM, said:

I am a potter of some years and have been working with a Grolleg cone 6 body for the last year or so. I am continually frustrated by bloating. The bisque has been totally fine tuned. The problem is with larger pieces - thrown from 8 to 14 lbs. Is this air trapped in the walls? out gasing? I am firing the schedule from the Cone 6 Glaze guys . . . I am making extra everything for orders to cover the losses. HELP!!



I've had this problem with a cone 6 brown body. Someone told me that the cause was bisqueing too fast so carbon didn't have time to escape. I changed to a very slow bisque and that seems to have done the trick, although I noticed a few bumps/bubbles on a recent load where I glaze fired very quickly so perhaps firing slowly all the time is the key. Good luck!
0

#5 User is offline   Denice Icon

  • Advanced Member
  • PipPipPip
  • Group: Members
  • Posts: 455
  • Joined: 02-April 10
  • LocationWichita, Kansas

Posted 10 January 2013 - 09:23 AM

I have been working with Cone 6 clays for 40 years the only time I have bloating is when I over fire. I'm a handbuilder mostly so I tend to fire slowly, I have noticed that some clays will bloat at Cone 7 so it doesn't take much. I learned this when I was learning how to use my dual pyrometer set to down fire and hold the temp in my kilns. Denice
0

#6 User is offline   Mark C. Icon

  • Advanced Member
  • PipPipPip
  • View gallery
  • Group: Members
  • Posts: 1,369
  • Joined: 09-January 12
  • LocationNear Arcata Ca-redwood rain forest

Posted 10 January 2013 - 11:50 AM

I'm guessing this is bloating not air bubbles-That comes from overfiring the clay body-one can also over reduce which can lead to bloating. If this is not the case and the clay is rated to cone 6 try bisquing a cone or two hotter. I see no connection to form size and bloating(small no bloat large bloat) unless the big pots are way thicker?
Mark
Mark Cortright
www.liscomhillpottery.com
0

#7 User is offline   mregecko Icon

  • Advanced Member
  • PipPipPip
  • Group: Members
  • Posts: 45
  • Joined: 14-November 12

Posted 10 January 2013 - 08:00 PM

I recently had a similar problem with a ^6 stoneware... Went through the theories of carbon coring, outgassing, air bubbles in clay, etc etc etc.

Come to find out my clay was just overspecced, and was in fact a ^5 clay. (Straight from the manufacturer's mouth)

I'd say try firing some pieces at a cone lower and see if you have the same problems.

Alternatively, you can bisque fire higher (04-02) and at a long cycle. Personally, I find that's A.) Annoying, and B.) Hard to glaze after.

Good luck, and let us know how things go!
0

#8 User is offline   Mark C. Icon

  • Advanced Member
  • PipPipPip
  • View gallery
  • Group: Members
  • Posts: 1,369
  • Joined: 09-January 12
  • LocationNear Arcata Ca-redwood rain forest

Posted 10 January 2013 - 10:34 PM

Many clay manufactures make cone 5 clay-but most seem to fire it to cone 6 it seems. One would think a cone 5 porcelain would take cone 6?
Mark
Mark Cortright
www.liscomhillpottery.com
0

#9 User is offline   OffCenter Icon

  • Advanced Member
  • PipPipPip
  • View gallery
  • Group: Members
  • Posts: 986
  • Joined: 01-April 10
  • LocationLizella, Georgia

Posted 11 January 2013 - 11:12 AM

View PostMark C., on 10 January 2013 - 10:34 PM, said:

Many clay manufactures make cone 5 clay-but most seem to fire it to cone 6 it seems. One would think a cone 5 porcelain would take cone 6?
Mark


I've tested a lot of them and never ran across a commercial cone 5 porcelain that wouldn't take cone 6. Pam hasn't replied yet so we don't even know that it is a commercial porcelain. If she mixes it herself, the problem may be in the mixing.

Jim
E pur si muove.

"But it does move," said Galileo under his breath.
0

#10 User is offline   neilestrick Icon

  • Neil Estrick
  • PipPipPip
  • Group: Members
  • Posts: 1,206
  • Joined: 04-October 11
  • LocationGrayslake, IL

Posted 11 January 2013 - 01:37 PM

View PostOffCenter, on 11 January 2013 - 10:12 AM, said:

I've tested a lot of them and never ran across a commercial cone 5 porcelain that wouldn't take cone 6.

Jim


I agree. Plus they usually have slumping problems before bloating shows up.
Neil Estrick
Kiln Repair Tech
L&L Distributor
Owner, Neil Estrick Gallery, LLC
www.neilestrickgallery.com

neil@neilestrickgallery.com
0

#11 User is offline   Wendey Icon

  • Member
  • PipPip
  • View gallery
  • Group: Members
  • Posts: 10
  • Joined: 23-March 12
  • LocationBurnaby, BC, Canada

Posted 13 January 2013 - 04:06 PM

Why do manufacturers make clays that fire to Cone 5 when most potters who make their own glazes fire to cone 6!????