Oops, too much water in the glaze. Reducing amount of water in glaze batch

#1 User is offline   Harry Potter Icon

  • Member
  • PipPip
  • Group: Members
  • Posts: 16
  • Joined: 12-June 12
  • LocationLouisiana and Mississippi

Posted 06 January 2013 - 12:14 AM

Well, here I am once again. Made a batch of Raku copper luster from book- alternative kilns and firing tech. Recipe notes from workshop noted batch made a gallon. Sooo I mixed up batch ( approx.1,060 grams) added a gallon of water, screened and it ended up very fluid. Any suggestions for reducing the amount of water or thickening up mix, I've already left top off hoping for evaporation. Aside from making up partial additional recipe to add to this batch, I'm at a loss.

Any suggestions? It's not like I could add flour to thicken it. But is there anything I could add to thicken without affecting the product. or just bite the bullet and make up partial recipe.

Recipe:
750.00 Gerstley borate

250.00 Bone

1000.00 Total

add

40.0 Copper carbonate

20.0 Cobalt Oxide
0

#2 User is offline   Pres Icon

  • Advanced Member
  • PipPipPip
  • View gallery
  • Group: Members
  • Posts: 994
  • Joined: 02-April 10
  • LocationCentral, PA

Posted 06 January 2013 - 12:24 AM

View PostHarry Potter, on 06 January 2013 - 12:14 AM, said:

Well, here I am once again. Made a batch of Raku copper luster from book- alternative kilns and firing tech. Recipe notes from workshop noted batch made a gallon. Sooo I mixed up batch ( approx.1,060 grams) added a gallon of water, screened and it ended up very fluid. Any suggestions for reducing the amount of water or thickening up mix, I've already left top off hoping for evaporation. Aside from making up partial additional recipe to add to this batch, I'm at a loss.

Any suggestions? It's not like I could add flour to thicken it. But is there anything I could add to thicken without affecting the product. or just bite the bullet and make up partial recipe.

Recipe:
750.00 Gerstley borate

250.00 Bone

1000.00 Total

add

40.0 Copper carbonate

20.0 Cobalt Oxide


Looks like too much clay to have much settling in the mix, otherwise I would pour off some water. Nope, can't think of anything else than maybe making up a 1/4 batch and adding to the present batch.
0

#3 User is offline   Mark C. Icon

  • Advanced Member
  • PipPipPip
  • View gallery
  • Group: Members
  • Posts: 1,360
  • Joined: 09-January 12
  • LocationNear Arcata Ca-redwood rain forest

Posted 06 January 2013 - 12:44 AM

Leave it alone for a day or three and with a small cup dip in so the water flows over the lip- just take the top water off and try to not disturb the reast-finish with a large sponge to get all the water.
All those materials will settle out in a few days. Evaporation takes too much time unless you live in Tucsan AZ and its summer time.
Mark
Mark Cortright
www.liscomhillpottery.com
0

#4 User is offline   yedrow Icon

  • Advanced Member
  • PipPipPip
  • View gallery
  • Group: Members
  • Posts: 362
  • Joined: 06-February 12

Posted 06 January 2013 - 01:12 AM

I've laid a box fan across the top, spaced with a couple of 2x4s.

Joel.
0

#5 User is offline   Iforgot Icon

  • Advanced Member
  • PipPipPip
  • View gallery
  • Group: Members
  • Posts: 137
  • Joined: 20-May 12
  • LocationColorado

Posted 06 January 2013 - 01:15 AM

I'd add two tablespoons of magnesium sulfate solution. if that turns out to be too much add like 4 tablespoons of majic water. or if it is just all settled in the bottom, which could be the problem you could add some cmc gum solution or bentonite.
Derek VonDrehle

Raku, Pit fired, Majolica, and Stoneware ceramic artisit
0

#6 User is offline   Harry Potter Icon

  • Member
  • PipPip
  • Group: Members
  • Posts: 16
  • Joined: 12-June 12
  • LocationLouisiana and Mississippi

Posted 06 January 2013 - 08:33 AM

I love this site, the members are so quick to respond. Good advice all the way around. I did try dipping in the mix and it seems to work, even if brushing seemed weak. May dip a couple of times to be sure thickness is sufficient. Thanks folks.
0

#7 User is offline   TJR Icon

  • Advanced Member
  • PipPipPip
  • View gallery
  • Group: Members
  • Posts: 698
  • Joined: 07-December 11
  • LocationCanada

Posted 06 January 2013 - 09:52 AM

Harry;
Mark is right. The simplest thing to do is let the batch sit for at least a day if not three, then decant the surface water without mixing up the rest. I would avoid adding anything else. I have on occaision added 3% bentonite. You have to mix it up with water in a small cup with a small amount of water. Then you have to re-sieve your entire glaze. A pain!
TJR
0

#8 User is online   OffCenter Icon

  • Advanced Member
  • PipPipPip
  • View gallery
  • Group: Members
  • Posts: 965
  • Joined: 01-April 10
  • LocationLizella, Georgia

Posted 06 January 2013 - 10:05 AM

View PostHarry Potter, on 06 January 2013 - 12:14 AM, said:

Well, here I am once again. Made a batch of Raku copper luster from book- alternative kilns and firing tech. Recipe notes from workshop noted batch made a gallon. Sooo I mixed up batch ( approx.1,060 grams) added a gallon of water, screened and it ended up very fluid. Any suggestions for reducing the amount of water or thickening up mix, I've already left top off hoping for evaporation. Aside from making up partial additional recipe to add to this batch, I'm at a loss.

Any suggestions? It's not like I could add flour to thicken it. But is there anything I could add to thicken without affecting the product. or just bite the bullet and make up partial recipe.

Recipe:
750.00 Gerstley borate

250.00 Bone

1000.00 Total

add

40.0 Copper carbonate

20.0 Cobalt Oxide


It's such a simple recipe, why don't you just divide each ingredient by 2 or 3 and add that to what you've already mixed up. Zap! problem solved without all that nonsense about waiting for water to evaporate.

Jim
E pur si muove.

"But it does move," said Galileo under his breath.
0

#9 User is offline   JBaymore Icon

  • Moderator
  • Icon
  • View gallery
  • Group: Moderators
  • Posts: 1,492
  • Joined: 06-April 10
  • LocationWilton, NH USA

Posted 06 January 2013 - 11:20 AM

View PostOffCenter, on 06 January 2013 - 10:05 AM, said:

It's such a simple recipe, why don't you just divide each ingredient by 2 or 3 and add that to what you've already mixed up. Zap! problem solved without all that nonsense about waiting for water to evaporate.


From my point of view this is THE answer. (Unless you are out of raw materials.)

best,

.............john
John Baymore
Immediate Past President; Potters Council
Professor of Ceramics; New Hampshire Insitute of Art

http://www.JohnBaymore.com
0

#10 User is offline   Chris Campbell Icon

  • Advanced Member
  • PipPipPip
  • View gallery
  • Group: Members
  • Posts: 1,367
  • Joined: 07-April 10
  • LocationRaleigh, NC

Posted 06 January 2013 - 12:17 PM

Another tip from a lazy potter ... I drape old cotton cloths around the bucket just letting the bottoms touch the surface. Through osmosis your cloths will be wet the next morning speeding up the evaporation process without much effort. I do this with my colored slips since they are easier to blend thin but I like to use them when they are thick.
Chris Campbell
Contemporary Fine Colored Porcelain
www.ccpottery.com

"My Artwork would not exist without a thriving global pottery community.
In the isolation of a studio, an artist can begin to feel like an island, but in truth
we are all part of archipelagoes; chains of islands loosely connected by a stream
of information that enhances our Artwork.”
1

#11 User is offline   yedrow Icon

  • Advanced Member
  • PipPipPip
  • View gallery
  • Group: Members
  • Posts: 362
  • Joined: 06-February 12

Posted 06 January 2013 - 02:09 PM

View PostChris Campbell, on 06 January 2013 - 12:17 PM, said:

Another tip from a lazy potter ... I drape old cotton cloths around the bucket just letting the bottoms touch the surface. Through osmosis your cloths will be wet the next morning speeding up the evaporation process without much effort. I do this with my colored slips since they are easier to blend thin but I like to use them when they are thick.