Porcelain Casting Slip Recipe Looking for a porcelain casting slip that I can mix myself.

#1 User is offline   TJR Icon

  • Advanced Member
  • PipPipPip
  • View gallery
  • Group: Members
  • Posts: 704
  • Joined: 07-December 11
  • LocationCanada

Posted 31 December 2012 - 03:26 PM

Hey, gang;
I am going to jump off the deep end and cast some porcelain in molds that I have made myself. I am a thrower, so this will be new for me, although I have seen it done. Any help would be appreciated.
And Happy New Year
TJR
CONE 10, SORRY!
0

#2 User is offline   OffCenter Icon

  • Advanced Member
  • PipPipPip
  • View gallery
  • Group: Members
  • Posts: 986
  • Joined: 01-April 10
  • LocationLizella, Georgia

Posted 31 December 2012 - 04:42 PM

View PostTJR, on 31 December 2012 - 03:26 PM, said:

Hey, gang;
I am going to jump off the deep end and cast some porcelain in molds that I have made myself. I am a thrower, so this will be new for me, although I have seen it done. Any help would be appreciated.
And Happy New Year
TJR


Hey TJR, I'm a thrower, too, so you'll probably get better info from people with more experience casting porcelain but I started casting the porcelains I throw with which is cone 6 Frost and cone 10 Southern Ice with a little paper in them. All I did was turn them into slip and add a little Darvon 7 to it. The white part with the colored circles in my (oh ######## I forgot what you call the little picture id thingy to the upper left of this post) is cast and it is paper thin and very translucent. So, if you throw porcelain you may want to consider using the same for casting.

Happy New Year!
Jim
E pur si muove.

"But it does move," said Galileo under his breath.
0

#3 User is offline   TJR Icon

  • Advanced Member
  • PipPipPip
  • View gallery
  • Group: Members
  • Posts: 704
  • Joined: 07-December 11
  • LocationCanada

Posted 31 December 2012 - 06:05 PM

View PostOffCenter, on 31 December 2012 - 03:42 PM, said:

View PostTJR, on 31 December 2012 - 03:26 PM, said:

Hey, gang;
I am going to jump off the deep end and cast some porcelain in molds that I have made myself. I am a thrower, so this will be new for me, although I have seen it done. Any help would be appreciated.
And Happy New Year
TJR


Hey TJR, I'm a thrower, too, so you'll probably get better info from people with more experience casting porcelain but I started casting the porcelains I throw with which is cone 6 Frost and cone 10 Southern Ice with a little paper in them. All I did was turn them into slip and add a little Darvon 7 to it. The white part with the colored circles in my (oh ######## I forgot what you call the little picture id thingy to the upper left of this post) is cast and it is paper thin and very translucent. So, if you throw porcelain you may want to consider using the same for casting.

Happy New Year!
Jim

Hey, offcentre;
Thanks for getting back to me so fast! I forgot to say Cone 10. I use a Plainsman clay called P580. I also use a stoneware from Laguna called Danish White. I am assuming just a couple of drops of Darvan7?
TJR.
0

#4 User is offline   Mark C. Icon

  • Advanced Member
  • PipPipPip
  • View gallery
  • Group: Members
  • Posts: 1,370
  • Joined: 09-January 12
  • LocationNear Arcata Ca-redwood rain forest

Posted 31 December 2012 - 06:07 PM

These slip is from my collage days but I used to use it.
Porc slip-
EPK-2.5#
Feldspar 2.5#
OM4 2.5#
Silica 2.5#
sodium sil 11.3 grams
add small amount of Darvon #7
water 4#s

I think this makes 1 gallon
Mark
Mark Cortright
www.liscomhillpottery.com
0

#5 User is offline   TJR Icon

  • Advanced Member
  • PipPipPip
  • View gallery
  • Group: Members
  • Posts: 704
  • Joined: 07-December 11
  • LocationCanada

Posted 31 December 2012 - 06:16 PM

View PostMark C., on 31 December 2012 - 05:07 PM, said:

These slip is from my collage days but I used to use it.
Porc slip-
EPK-2.5#
Feldspar 2.5#
OM4 2.5#
Silica 2.5#
sodium sil 11/3 grams
add small amount of Darvon #7
water 4#s

I think this makes 1 gallon
Mark


THANKS, MATE.
Tom.
0

#6 User is offline   Mark C. Icon

  • Advanced Member
  • PipPipPip
  • View gallery
  • Group: Members
  • Posts: 1,370
  • Joined: 09-January 12
  • LocationNear Arcata Ca-redwood rain forest

Posted 31 December 2012 - 06:26 PM

I edited the sodium sill amount-check it out.
Mark
Mark Cortright
www.liscomhillpottery.com
0

#7 User is offline   TJR Icon

  • Advanced Member
  • PipPipPip
  • View gallery
  • Group: Members
  • Posts: 704
  • Joined: 07-December 11
  • LocationCanada

Posted 31 December 2012 - 06:33 PM

View PostMark C., on 31 December 2012 - 05:26 PM, said:

I edited the sodium sill amount-check it out.
Mark


Mark;
So everything is in pounds except the sodiun silicate. Is that correct?
Tom.
0

#8 User is offline   Mark C. Icon

  • Advanced Member
  • PipPipPip
  • View gallery
  • Group: Members
  • Posts: 1,370
  • Joined: 09-January 12
  • LocationNear Arcata Ca-redwood rain forest

Posted 31 December 2012 - 08:33 PM

Yes thats right.
this recipe is very simple-it used to call or soda ash but Darvon is better on the plaster.
Timing this with a slip cup is also a good idea to tune it up.
Mark
Mark Cortright
www.liscomhillpottery.com
0