Firing large piece? Rate Topic: -----

#1 User is offline   CPT Icon

  • Advanced Member
  • PipPipPip
  • Group: Members
  • Posts: 45
  • Joined: 07-February 12

Posted 11 November 2012 - 10:01 AM

Hi Everyone:

I'm stuck on what to do here. I will be decorating this rather large bisqueware bread platter just on the top portion (24" L) and then glaze fire to Cone 06. Trouble is, I can only set it at an angle in my little kiln.

Can I do this? Will this piece be ok touching the sides of the fire brick?

Thanks for your advice in advance.

Attached File(s)


0

#2 User is offline   Denice Icon

  • Advanced Member
  • PipPipPip
  • Group: Members
  • Posts: 455
  • Joined: 02-April 10
  • LocationWichita, Kansas

Posted 11 November 2012 - 11:12 AM

I think having it that close to a coil could cause many problems over fiing, glaze changes even cracking because of uneven shrinkage and you would have to use a real stable glaze. It looks like you could put a piece of bisque ware to lean it against to get it away from the wall. If I get carried away with size I take it to a ceramic supply store that does firing, I know that most people aren't that lucky to have a retail buisness like that near by. Good Luck Denice
0

#3 User is offline   CPT Icon

  • Advanced Member
  • PipPipPip
  • Group: Members
  • Posts: 45
  • Joined: 07-February 12

Posted 11 November 2012 - 12:01 PM

Thanks Denice:

I'll keep looking around. I may look into a kiln timeshare with someone.

This is so frustrating.....

http://www.bigcerami...timesharing.htm
0

#4 User is offline   neilestrick Icon

  • Neil Estrick
  • PipPipPip
  • Group: Members
  • Posts: 1,206
  • Joined: 04-October 11
  • LocationGrayslake, IL

Posted 11 November 2012 - 02:09 PM

That would be bad to have it against the side of the kiln. Search for someone with a big enough kiln for it.
Neil Estrick
Kiln Repair Tech
L&L Distributor
Owner, Neil Estrick Gallery, LLC
www.neilestrickgallery.com

neil@neilestrickgallery.com
0

#5 User is offline   Benzine Icon

  • Advanced Member
  • PipPipPip
  • Group: Members
  • Posts: 374
  • Joined: 08-September 12

Posted 11 November 2012 - 04:29 PM

Perhaps, if time isn't a factor, build some type of holder out of clay, that would hold the platter at an angle, but not touching the kiln walls, or even more vertically. Build it, bisque it, and there you go.
"Anything worth believing, is worth questioning"
0

#6 User is offline   Marcia Selsor Icon

  • Advanced member
  • PipPipPip
  • View gallery
  • Group: Members
  • Posts: 2,453
  • Joined: 16-May 10
  • LocationBrownsville, TX

Posted 11 November 2012 - 10:21 PM

I have often said Ceramics is only limited by your imagination and the size of your kiln.
I hope yo find a way to fire tha t piece...or in the future you need a bigger kiln.
Best wishes,
Marcia
Marcia Selsor
0

#7 User is offline   JLowes Icon

  • Clay Doodler
  • PipPipPip
  • View gallery
  • Group: Members
  • Posts: 133
  • Joined: 01-June 10
  • LocationAtlanta Georgia area

Posted 12 November 2012 - 04:51 PM

I didn't have as extreme an example as yours, but I had a piece that I wanted to fire in my smaller kiln rather than having a lot of empty space in my larger kiln. So, I propped it on an angle blocked up and supported so it couldn't move around during firing. Not having to worry about glaze on the bottom may allow you to do something like that. Mine did NOT touch the walls, but was very close. The Cone 06 is in your favor. Still, if you can find a place to fire it normally would be the best.

John
0

#8 User is offline   SmartsyArtsy Icon

  • Chris Seminara
  • PipPipPip
  • View gallery
  • Group: Members
  • Posts: 143
  • Joined: 29-October 11
  • LocationPNW

Posted 13 November 2012 - 11:56 PM

I recently used my tall kiln posts to prop up a "got carried away and made it too long" piece. It wasn't a critical form, though, so I didn't worry about warping. I would find a larger kiln for your piece.


Chris
Chris Seminara Ceramics
Member, Artisan Tile NorthWest
0

#9 User is offline   perkolator Icon

  • Advanced Member
  • PipPipPip
  • Group: Members
  • Posts: 179
  • Joined: 08-February 12
  • LocationCalifornia

Posted 14 November 2012 - 08:05 PM

i fire pieces like that all the time. i don't do it often and it's usually just test tiles to test flow of the glaze -- and it will most likely warp unless it's fully supported across the bottom of the form. there's also the concern that your glaze decoration might shift because of the vertical position. another problem with supporting a piece such as this, is that you'll have to leave a bare spot where it contacts the floor shelves and wall of kiln, or use bar stilt.

i've got lots of shelf shapes/sizes to play around with supporting pieces like this, but for you you'd most likely have to construct a support like Benzine and others have mentioned. if well supported, there shouldn't be much pressure on the soft brick wall so the only real concern there would be glaze sticking to it if it's touching.

safest way is find someone with a larger kiln.
0

#10 User is offline   Pres Icon

  • Advanced Member
  • PipPipPip
  • View gallery
  • Group: Members
  • Posts: 997
  • Joined: 02-April 10
  • LocationCentral, PA

Posted 15 November 2012 - 10:53 AM

View PostCPT, on 11 November 2012 - 10:01 AM, said:

Hi Everyone:

I'm stuck on what to do here. I will be decorating this rather large bisqueware bread platter just on the top portion (24" L) and then glaze fire to Cone 06. Trouble is, I can only set it at an angle in my little kiln.

Can I do this? Will this piece be ok touching the sides of the fire brick?

Thanks for your advice in advance.


I have seen someone fire this type of thing once in a small electric kiln. They made a wedge shaped foundation of soft fire brick that had a stop edge at the bottom where the piece did not touch the kiln floor. It was completely supported on the wedge shaped firebrick. They did not glaze the outside of the piece only stained it. You have a definite problem-good luck.
0

#11 User is offline   ClayByMck Icon

  • Newbie
  • Pip
  • Group: Members
  • Posts: 4
  • Joined: 02-December 12

Posted 02 December 2012 - 08:58 PM

Easy! lol. Heres the solution. You are only up against warping, glaze running everywhere, staining from the backside being unfinished and worst of all, breaking in half and sticking to your evements and bricks, but heres an idea. From my experience I would lay it face down on a pillow. Use a dremmel, hack saw, or metal file to score an interesting line down middle short-wise. Be sure to make the score deeper where the footing rises. Leaving it face down on the pillow, tap the score line with a hammer. I would tap first on the footing. You will have 2 beautiful 12 inch beautifully finished pieces to attach after theyre fired. I would stylize the line where the two pieces meet with a fancy painted border to make the break look intentional. While breaking your beloved platter in half may not be fun. It will be liberating. Good luck. Hope to see pics.
0