: Matte glazes -

Jump to content

Share Topic:   facebook stumbleupon del-icio-us digg email google mixx reddit
Page 1 of 1
  • You cannot start a new topic
  • You cannot reply to this topic

Matte glazes matte glaze that allows RIO to show through

#1 User is offline   elainecarroll Icon

  • Newbie
  • Pip
  • Group: Members
  • Posts: 4
  • Joined: 24-October 11
  • LocationBaton Rouge, LA

Posted 05 November 2012 - 01:52 PM

I am very new to making glazes and would really appreciate some help. I am looking for some matte glaze recipes that would allow red iron oxide to show through. If anyone can point me in the right direction, I surely would appreciate it. Thanks Elaine
0

#2 User is offline   neilestrick Icon

  • Neil Estrick
  • PipPipPip
  • Group: Members
  • Posts: 1,204
  • Joined: 04-October 11
  • LocationGrayslake, IL

Posted 05 November 2012 - 05:54 PM

Firing to what cone and atmosphere?
Neil Estrick
Kiln Repair Tech
L&L Distributor
Owner, Neil Estrick Gallery, LLC
www.neilestrickgallery.com

neil@neilestrickgallery.com
0

#3 User is offline   elainecarroll Icon

  • Newbie
  • Pip
  • Group: Members
  • Posts: 4
  • Joined: 24-October 11
  • LocationBaton Rouge, LA

Posted 05 November 2012 - 08:37 PM

View Postneilestrick, on 05 November 2012 - 05:54 PM, said:

Firing to what cone and atmosphere?

Sorry, Cone 6 oxidation
0

#4 User is offline   neilestrick Icon

  • Neil Estrick
  • PipPipPip
  • Group: Members
  • Posts: 1,204
  • Joined: 04-October 11
  • LocationGrayslake, IL

Posted 06 November 2012 - 01:29 PM

To get iron to show through in cone 6 oxidation, it takes a lot more iron than in reduction. I used to use a 10% iron slip in reduction, but use 20% iron in oxidation. Whether you're using a slip or straight iron oxide, it will show through most matte glazes if the iron/slip is thick enough. Glazes that are matte due due crystal growth rather than due to under-firing will tend to show it more because it will get into the melt more. Test, test, test....
Neil Estrick
Kiln Repair Tech
L&L Distributor
Owner, Neil Estrick Gallery, LLC
www.neilestrickgallery.com

neil@neilestrickgallery.com
0

#5 User is offline   elainecarroll Icon

  • Newbie
  • Pip
  • Group: Members
  • Posts: 4
  • Joined: 24-October 11
  • LocationBaton Rouge, LA

Posted 06 November 2012 - 06:56 PM

View Postneilestrick, on 06 November 2012 - 01:29 PM, said:

To get iron to show through in cone 6 oxidation, it takes a lot more iron than in reduction. I used to use a 10% iron slip in reduction, but use 20% iron in oxidation. Whether you're using a slip or straight iron oxide, it will show through most matte glazes if the iron/slip is thick enough. Glazes that are matte due due crystal growth rather than due to under-firing will tend to show it more because it will get into the melt more. Test, test, test....

Thanks so much, that is exactly the info I needed. I will start testing.