Using a sieve for glazes Reasons for using a sieve (screen) for glazes

#1 User is offline   kelleyisfj Icon

  • Member
  • PipPip
  • Group: Members
  • Posts: 10
  • Joined: 14-May 10
  • LocationOakland, CA

Posted 13 October 2012 - 03:24 AM

I'd like to hear some compelling reasons for using a sieve for making glazes.
0

#2 User is offline   weeble Icon

  • Advanced Member
  • PipPipPip
  • View gallery
  • Group: Members
  • Posts: 95
  • Joined: 12-August 12
  • LocationOregon Coast

Posted 13 October 2012 - 04:41 AM

Lumps.
Maryjane Carlson

Whistling Fish Pottery
0

#3 User is offline   neilestrick Icon

  • Neil Estrick
  • PipPipPip
  • Group: Members
  • Posts: 1,191
  • Joined: 04-October 11
  • LocationGrayslake, IL

Posted 13 October 2012 - 08:50 AM

Gets out the lumps. A mixer won't cut it, unless you have a high shear industrial mixer....
Neil Estrick
Kiln Repair Tech
L&L Distributor
Owner, Neil Estrick Gallery, LLC
www.neilestrickgallery.com

neil@neilestrickgallery.com
0

#4 User is offline   JBaymore Icon

  • Moderator
  • Icon
  • View gallery
  • Group: Moderators
  • Posts: 1,484
  • Joined: 06-April 10
  • LocationWilton, NH USA

Posted 13 October 2012 - 09:32 AM

Most compelling is that if you want your glazes (typically) to look good, seiving assures that. Consistency.

best,

.......................john
John Baymore
Immediate Past President; Potters Council
Professor of Ceramics; New Hampshire Insitute of Art

http://www.JohnBaymore.com
0

#5 User is offline   Nelly Icon

  • Advanced Member
  • PipPipPip
  • Group: Members
  • Posts: 368
  • Joined: 20-February 12

Posted 13 October 2012 - 02:53 PM

View PostJBaymore, on 13 October 2012 - 09:32 AM, said:

Most compelling is that if you want your glazes (typically) to look good, seiving assures that. Consistency.

best,

.......................john



Dear All,

I totally agree with all that has been said. Grit. Lumps that somehow get into the glaze and you don't notice them until they are smack gob on the middle of your pot after firing. When at all possible I like to seive before I dip or pour. Then I gently review the piece looking for little air bubbles. I smooth these out as well. Any cracks in the glaze from big gobs I scrape off and start again.

And I think the taliman seive is a great invention. I recall the days we painted glazed through seives with brush. It was hard work. If you don't have one a talisman is great for the initial mixing. I used the wire strainers you can get from the dollar store when it comes to seiving smaller amounts.

Nelly
0

#6 User is offline   JBaymore Icon

  • Moderator
  • Icon
  • View gallery
  • Group: Moderators
  • Posts: 1,484
  • Joined: 06-April 10
  • LocationWilton, NH USA

Posted 13 October 2012 - 03:59 PM

View PostNelly, on 13 October 2012 - 03:53 PM, said:

And I think the taliman seive is a great invention.



+1

John Baymore
Immediate Past President; Potters Council
Professor of Ceramics; New Hampshire Insitute of Art

http://www.JohnBaymore.com
0

#7 User is offline   Marcia Selsor Icon

  • Advanced member
  • PipPipPip
  • View gallery
  • Group: Members
  • Posts: 2,431
  • Joined: 16-May 10
  • LocationBrownsville, TX

Posted 14 October 2012 - 12:28 AM

yep. lumps. Ugly white ones. I was a guest artist at a center recently and used the center's glaze as part of prepping for a firing demo. it was not sieved. Got awful lumps on a very large bowl.
I tried refiring it when I got home but you can't cover up those lumps.
Marcia
Marcia Selsor
0

#8 User is offline   Kohaku Icon

  • Advanced Member
  • PipPipPip
  • Group: Members
  • Posts: 83
  • Joined: 12-October 12
  • LocationMoscow, Idaho

Posted 14 October 2012 - 09:17 AM

Not just lumps, but general distribution of ingredients. You can get streakiness, blotchiness, color variation... or even faults like crawling in some cases.

I once skipped the sieve step with a glaze that was heavy on the copper oxide (just wielded the mixer like madman). It looked OK in the bucket, but gave the most oddball, variegated effects I'd ever seem. Not even displeasing... but totally unpredictable.
Not all who wander are lost
0

#9 User is offline   Denice Icon

  • Advanced Member
  • PipPipPip
  • Group: Members
  • Posts: 450
  • Joined: 02-April 10
  • LocationWichita, Kansas

Posted 14 October 2012 - 10:53 AM

Can''t imagine making glazes without sieves, I have a small one for test glazes and a bowl type for larger batches. The larger one is about 30 year old and is starting to wear out I keep patching it with silicone. I'm turning 60 Monday so I think I'm going to treat myself and order a talisman. Denice
0

#10 User is offline   JBaymore Icon

  • Moderator
  • Icon
  • View gallery
  • Group: Moderators
  • Posts: 1,484
  • Joined: 06-April 10
  • LocationWilton, NH USA

Posted 14 October 2012 - 11:58 AM

View PostDenice, on 14 October 2012 - 11:53 AM, said:

I'm turning 60 Monday so I think I'm going to treat myself and order a talisman.


Happy Birthday, Denise.

And you won't go wrong wit hthe Tallisman seive. Altjough I wish they still made the body of aluminum (I have one of each).

best,

..............john
John Baymore
Immediate Past President; Potters Council
Professor of Ceramics; New Hampshire Insitute of Art

http://www.JohnBaymore.com
0

#11 User is offline   TJR Icon

  • Advanced Member
  • PipPipPip
  • View gallery
  • Group: Members
  • Posts: 695
  • Joined: 07-December 11
  • LocationCanada

Posted 14 October 2012 - 05:58 PM

I sieve all of my glazes every time I go to glaze. I sieve first through an 80 mesh sieve, wash the 5 gallon bucket, then sieve the glaze back into the original bucket through a 100 mesh sieve.
If you don't sieve, you have lumps and inconsistency of texture.
Go buy a sieve.I can't believe I used the word sieve eight times.
TJR.
0

#12 User is offline   TJR Icon

  • Advanced Member
  • PipPipPip
  • View gallery
  • Group: Members
  • Posts: 695
  • Joined: 07-December 11
  • LocationCanada

Posted 14 October 2012 - 05:58 PM

I sieve all of my glazes every time I go to glaze. I sieve first through an 80 mesh sieve, wash the 5 gallon bucket, then sieve the glaze back into the original bucket through a 100 mesh sieve.
If you don't sieve, you have lumps and inconsistency of texture.
Go buy a sieve.I can't believe I used the word sieve eight times.
TJR.
0

#13 User is offline   bciskepottery Icon

  • Advanced Member
  • PipPipPip
  • Group: Members
  • Posts: 753
  • Joined: 28-June 10

Posted 14 October 2012 - 07:42 PM

As I was mixing a new batch of slip this afternoon and using a scrub brush to work the slip through a 60 mesh sieve, this discussion of the benefits of a Talisman kept ringing in my mind.
0

#14 User is offline   Mark C. Icon

  • Advanced Member
  • PipPipPip
  • View gallery
  • Group: Members
  • Posts: 1,353
  • Joined: 09-January 12
  • LocationNear Arcata Ca-redwood rain forest

Posted 15 October 2012 - 07:49 PM

Talisman 80 mesh for me-everything goes thru it and all is well afterwards.
I have all the screen sizes but long ago found the 80 to be enough for 99.9% of needs-now after wearing out 3 of them its still true.
The big labor savers are when clay is your livelihood
pre made clay
power wheel
Talisman sieve
Power mixer for glazes
car kiln
electric slab roller
I wish I had them all when I was younger-or at least my body does.
Mark
Mark Cortright
www.liscomhillpottery.com
0

#15 User is offline   Idaho Potter Icon

  • Advanced Member
  • PipPipPip
  • View gallery
  • Group: Members
  • Posts: 305
  • Joined: 26-August 10
  • LocationBoise, Idaho

Posted 16 October 2012 - 07:00 PM

If a glaze hasn't been used in awhile, it should be sieved before using because ingredients tend to clump and lump if left undisturbed. I was laughed at for sieving my raku glazes ( I guess because so many of them are made using borax) but running the glaze through a screen mixes everything well, and if there are small particles (usually crystalline) I use the last of the mixing water to rinse them back into the mix, so I lose nothing.