White semi-opaque cone 6 glaze? Looking for a white-wash looking glaze

#1 User is offline   JRWebb Pottery Icon

  • Member
  • PipPip
  • Group: Members
  • Posts: 10
  • Joined: 05-August 11

Posted 02 May 2012 - 02:41 PM

I am looking for either a commercial glaze or a simple glaze recipe that will look sorta like white-washing.
It can be semi-opaque, but I want to see the texture through it. Can be either satin or gloss finish.

I work with white stoneware clay and fire to cone 6.

Anyone have some ideas?

Thanks! Jonni
0

#2 User is online   Mark C. Icon

  • Advanced Member
  • PipPipPip
  • View gallery
  • Group: Members
  • Posts: 1,349
  • Joined: 09-January 12
  • LocationNear Arcata Ca-redwood rain forest

Posted 03 May 2012 - 01:25 AM

Google
White semi-opaque cone 6 glaze?
the 3rd hit is a Vangilder pdf with your glazes
Mark
Mark Cortright
www.liscomhillpottery.com
0

#3 User is offline   JRWebb Pottery Icon

  • Member
  • PipPip
  • Group: Members
  • Posts: 10
  • Joined: 05-August 11

Posted 05 May 2012 - 08:52 PM

View PostMark C., on 03 May 2012 - 12:25 AM, said:

Google
White semi-opaque cone 6 glaze?
the 3rd hit is a Vangilder pdf with your glazes
Mark



Thanks a bunch!!
0

#4 User is offline   Marcia Selsor Icon

  • Advanced member
  • PipPipPip
  • View gallery
  • Group: Members
  • Posts: 2,419
  • Joined: 16-May 10
  • LocationBrownsville, TX

Posted 06 May 2012 - 07:51 AM

This is one I used in reduction for decades



WAXY WHITE (^6 OX)




Custer feldspar 41

Silica 20

Talc 15

Gerstley Borate 15

Dolomite 7

EPK 5

103




Marcia








Marcia Selsor
0

#5 User is offline   JRWebb Pottery Icon

  • Member
  • PipPip
  • Group: Members
  • Posts: 10
  • Joined: 05-August 11

Posted 06 May 2012 - 08:19 AM

View PostMarcia Selsor, on 06 May 2012 - 06:51 AM, said:

This is one I used in reduction for decades



WAXY WHITE (^6 OX)




Custer feldspar 41

Silica 20

Talc 15

Gerstley Borate 15

Dolomite 7

EPK 5

103




Marcia



Thank you, Marcia! I'm going to mix it up and give that one a try today!