Solid Glaze Glaze solidifies at the bottom of the bucket?

#1 User is offline   Elmoclayman Icon

  • Member
  • PipPip
  • Group: Members
  • Posts: 14
  • Joined: 19-April 12

Posted 19 April 2012 - 01:11 PM

I teach a high school ceramics class and I have noticed that a couple of my glazes (stored in 5 gallon buckets), solidify at the bottom of the bucket if they sit over night. I have to drain the liquid off, then chip away at the "solid" glaze material, then remix the glaze. It is very time consuming. Is there a material I can add to my glazes to prevent this without altering the color of the glaze?

Thanks in advance
0

#2 User is offline   Matt Oz Icon

  • Advanced Procrastinator
  • PipPipPip
  • View gallery
  • Group: Members
  • Posts: 206
  • Joined: 16-December 11

Posted 19 April 2012 - 01:52 PM

You'll get lots of good advice here, in the meantime here is a popular article on the subject.

Adjusting Glazes for Application by Pete Pinnell
0

#3 User is offline   Pres Icon

  • Advanced Member
  • Icon
  • View gallery
  • Group: Moderators
  • Posts: 1,097
  • Joined: 02-April 10
  • LocationCentral, PA

Posted 19 April 2012 - 01:53 PM

View PostElmoclayman, on 19 April 2012 - 01:11 PM, said:

I teach a high school ceramics class and I have noticed that a couple of my glazes (stored in 5 gallon buckets), solidify at the bottom of the bucket if they sit over night. I have to drain the liquid off, then chip away at the "solid" glaze material, then remix the glaze. It is very time consuming. Is there a material I can add to my glazes to prevent this without altering the color of the glaze?

Thanks in advance


This usually happens when the clay content in the glaze is low. I used to have a gallon jar in the classroom of Epsom Salts dissolved in water(dissolve as much as you can without residue). a couple of tablespoons of this would deflocculate the glaze and make it stay i suspension longer. Others use things like gum Arabic, but as that is organic, it will grow mold. Bentonite can be added to the glaze in small percentages to help with this also.
0

#4 User is online   Mark C. Icon

  • Advanced Member
  • PipPipPip
  • View gallery
  • Group: Members
  • Posts: 1,436
  • Joined: 09-January 12
  • LocationNear Arcata Ca-redwood rain forest

Posted 19 April 2012 - 02:40 PM

What Pres said
Epsom Salts dissolved in warm water-add to glaze after you have poured off some water and remixed all the solids.
If this is not enough to keep it suspended there are other ways as well but are a bit more costly and more work.
Mark
Mark Cortright
www.liscomhillpottery.com
0

#5 User is offline   Marcia Selsor Icon

  • Advanced member
  • PipPipPip
  • View gallery
  • Group: Members
  • Posts: 2,500
  • Joined: 16-May 10
  • LocationBrownsville, TX

Posted 19 April 2012 - 02:50 PM

Yep. Epsom salts. I put it in when I first mix the glaze if it is prone to doing that.
Marcia
Marcia Selsor
0

#6 User is offline   TJR Icon

  • Advanced Member
  • PipPipPip
  • View gallery
  • Group: Members
  • Posts: 739
  • Joined: 07-December 11
  • LocationCanada

Posted 19 April 2012 - 03:16 PM

I use 2% Bentonite if the glaze does not have much clay in it. Mix in hot water first, then dump in the glaze bucket.You will have to mix quite well. For 5 gallons og glaze you would need 100 grams of Bentonite.