base:

silica 2
3124 89.5
epk 8.5
bentonite 2
vgum 1tsp

10% #6008 peach mason stain

fired to cone 06.

its supposed to be a medium-dark peach, but came out baby pink.

any suggestions?
www.lotsapotsa.com
www.daddyzero.com
0

#2 User is offline   Nelly Icon

  • Advanced Member
  • PipPipPip
  • Group: Members
  • Posts: 379
  • Joined: 20-February 12

Posted 15 April 2012 - 12:52 PM

View Postmissholly, on 15 April 2012 - 11:34 AM, said:

base:

silica 2
3124 89.5
epk 8.5
bentonite 2
vgum 1tsp

10% #6008 peach mason stain

fired to cone 06.

its supposed to be a medium-dark peach, but came out baby pink.

any suggestions?


Dear All,

I have used peach colored mason stain but I always mix it with slip. I use Robin Hoppers slip recipe. I was told that the color of slip is always enhanced if you first put a white colored plain slip down and then the colored one. It has worked for me on Plainsmen's darkest red cone 6 clay.

Nellie
0

#3 User is offline   missholly Icon

  • Advanced Member
  • PipPipPip
  • Group: Members
  • Posts: 158
  • Joined: 14-December 10
  • Locationzanesville, ohio

Posted 16 April 2012 - 06:16 PM

my clay is white.
www.lotsapotsa.com
www.daddyzero.com
0

#4 User is offline   bciskepottery Icon

  • Advanced Member
  • PipPipPip
  • Group: Members
  • Posts: 753
  • Joined: 28-June 10

Posted 16 April 2012 - 06:41 PM

Consider adding more stain to the glaze; 10% might not be enough.
0

#5 User is offline   neilestrick Icon

  • Neil Estrick
  • PipPipPip
  • Group: Members
  • Posts: 1,239
  • Joined: 04-October 11
  • LocationGrayslake, IL

Posted 17 April 2012 - 04:16 PM

According to the Mason Reference chart: 9. Glaze must contain 6.7 to 8.4% CaO (12-15% CaCO3). Your glaze is at 12.8%, so a bit high. I would try a different base, or try fiddling with that recipe. It's a tough one to alter without messing it up, though.
Neil Estrick
Kiln Repair Tech
L&L Distributor
Owner, Neil Estrick Gallery, LLC
www.neilestrickgallery.com

neil@neilestrickgallery.com
0

#6 User is offline   missholly Icon

  • Advanced Member
  • PipPipPip
  • Group: Members
  • Posts: 158
  • Joined: 14-December 10
  • Locationzanesville, ohio

Posted 18 April 2012 - 07:18 AM

ive used other stains with this base and they worked out fine.
ill up the percentage and see what happens.

thanks guys!
www.lotsapotsa.com
www.daddyzero.com
0

#7 User is offline   Marcia Selsor Icon

  • Advanced member
  • PipPipPip
  • View gallery
  • Group: Members
  • Posts: 2,500
  • Joined: 16-May 10
  • LocationBrownsville, TX

Posted 21 April 2012 - 07:34 AM

Here is the Clear ^6 I use with stains. It works really well with crimson Mason Stains. Please forgive the formatting. This is a nice smooth satin to shiny clear.
It is high in Calcium Carb, but it is the same code for crimson and it works well there.
Sue Hintz Clear 6^ reworked by Ron Roy back in late 90s.



Cornwall Stone 33.5

G200 22
Whiting 18
Gerstley Borate 10
EPKaolin 5.5
Silica 11
Bentonite 2

Marcia