Problem with making hollow extrusions how to get them even?
#1
Posted 25 February 2012 - 09:56 AM
the sides of the extrusion collapse inward and the entire pieces curls upward. I'm having my partner pull the handle and I sit under the barrel and pull and stretch on the exiting clay, trying to get it straight. The sides of the extruded piece are uneven, one side is twice as thick as the other, no matter how straight I start the center die piece.
The problem is the same with softer, harder and well wedged clay. None of that makes it better.
Any suggestions will be appreciated.
#2
Posted 25 February 2012 - 10:20 AM
The extrusions should come out with all sides even if the die has even sides. The beginning few inches tend to curl up but the weight should then make the extrusion fall straight. You should not have to pull it at all ... I only guide mine and take some of the weight.
I would call the manufacturer and ask for some tech support.
Contemporary Fine Colored Porcelain
www.ccpottery.com
"My Artwork would not exist without a thriving global pottery community.
In the isolation of a studio, an artist can begin to feel like an island, but in truth
we are all part of archipelagoes; chains of islands loosely connected by a stream
of information that enhances our Artwork.”
#3
Posted 25 February 2012 - 10:42 AM
Chris Campbell, on 25 February 2012 - 10:20 AM, said:
The extrusions should come out with all sides even if the die has even sides. The beginning few inches tend to curl up but the weight should then make the extrusion fall straight. You should not have to pull it at all ... I only guide mine and take some of the weight.
I would call the manufacturer and ask for some tech support.
I did and I was told it would get better with practice. Well and good, but I've practiced, hung upside down under it, cursed, put shims in the housing trying to hold it more stable and therefore unmovable. I start out with the center piece even in the housing and as soon as the clay comes through, it goes off center enough to cause a difference in the wall thickness, hence the crookedness to my way of understanding.
After some close examination, I discovered the center post that holds the center die was not evenly set in the center die hanger,so I called them asking if they had a straighter one. I was sent one some better and the problem improved slightly.
I'm still working and over handling little hollow pieces and truly fighting to get larger pieces to be usable. I bought the 5" to be able to make larger work, but the crookedness has an even greater effect on larger works.
I'm hoping someone with lots of extruder time will have a suggestion.
#4
Posted 25 February 2012 - 01:39 PM
clay lover, on 25 February 2012 - 10:42 AM, said:
Chris Campbell, on 25 February 2012 - 10:20 AM, said:
The extrusions should come out with all sides even if the die has even sides. The beginning few inches tend to curl up but the weight should then make the extrusion fall straight. You should not have to pull it at all ... I only guide mine and take some of the weight.
I would call the manufacturer and ask for some tech support.
I did and I was told it would get better with practice. Well and good, but I've practiced, hung upside down under it, cursed, put shims in the housing trying to hold it more stable and therefore unmovable. I start out with the center piece even in the housing and as soon as the clay comes through, it goes off center enough to cause a difference in the wall thickness, hence the crookedness to my way of understanding.
After some close examination, I discovered the center post that holds the center die was not evenly set in the center die hanger,so I called them asking if they had a straighter one. I was sent one some better and the problem improved slightly.
I'm still working and over handling little hollow pieces and truly fighting to get larger pieces to be usable. I bought the 5" to be able to make larger work, but the crookedness has an even greater effect on larger works.
I'm hoping someone with lots of extruder time will have a suggestion.
I have an older scott creek 4 inch barrel-I have not made hollow stuff for years but did at one time. The center hole is a 3 legged tripod which you can spread the legs so that they are against the barrel and is in center and cannot move- when the cap is on.
What ever the system that puts the center die in center( it will not be the same 3 legs for a square barrel) make sure it cannot shift as thats what causes the uneven wall thickness you are experiencing.
I looked at this model and the hollow core shapes on the web but no where was the center holder shown-so I cannot see how it works.
One tip is I like to spray with mist the setup as its starts.
Mark
www.liscomhillpottery.com
#6 Guest_The Unknown Craftsman_*
Posted 25 February 2012 - 02:20 PM


It appears that the tripod is used in the round barrel extruders, and not in the square barrel models, which claylover has.
"I start out with the center piece even in the housing and as soon as the clay comes through, it goes off center enough to cause a difference in the wall thickness, hence the crookedness to my way of understanding."
Do you mean the center piece of the die goes off center, or the clay?
Is this happening consistently, is the thicker wall always on the same side of every extrusion, or does it change from extrusion to extrusion?
#7
Posted 25 February 2012 - 02:55 PM
The Unknown Craftsman, on 25 February 2012 - 02:20 PM, said:


It appears that the tripod is used in the round barrel extruders, and not in the square barrel models, which claylover has.
"I start out with the center piece even in the housing and as soon as the clay comes through, it goes off center enough to cause a difference in the wall thickness, hence the crookedness to my way of understanding."
Do you mean the center piece of the die goes off center, or the clay?
Is this happening consistently, is the thicker wall always on the same side of every extrusion, or does it change from extrusion to extrusion?
That square jig looks to have some play in it side to side-looks like a few shims will fix that.It needs to not be able to move any direction.
On a whole other note that round barel jig look nothing like my scott creek one from the 70's
Mark
www.liscomhillpottery.com
#8 Guest_The Unknown Craftsman_*
Posted 25 February 2012 - 03:01 PM
That was my thinking at first, too, Mark, but then I noticed that the barrel and the bridge have holes in them, into which fit the quick release pins; so the bridge really should be centered and held firm. I say "should..."
#10
Posted 25 February 2012 - 04:22 PM
Mark C., on 25 February 2012 - 03:18 PM, said:
Mark
There is MUCH play in the housing set up. Scott Creek rep says that is necessary for the assembly to be user friendly???
The washer is tight. I used shims yesterday both inside and outside the square collaring that holds it all in place, didn't make any improvement to outcomes. I can't figure out how the center die could shift when extruding, with all the play in the collar taken up with solid shims, but it did. I hang upside down look and measure spacing all around the center die, it looks centered, then I extrude clay and the walls are uneven and the extrusion twists and curls. I'm ready to give up and sell it.
I am hoping someone on here with the same item, 5" Scot Creek, will come back with some advice.
Yes, there are 4 cotter [pins spaced evenly around the 2 sides of the square collar, they fit through the center die support which is an H shaped heavy aluminum device.
#11
Posted 25 February 2012 - 04:42 PM
How about when you are starting to extrude you hod the extrusion in hand and guide it straight down . You may have to let it curl a little first-also one last item
The plane where the washer sits is very important-if its to high up or to low as compared to the outer plate this will cause problems-should be about flush with outer dies.
I think just a little fine tuning will fix this-
Mark
www.liscomhillpottery.com
#12 Guest_The Unknown Craftsman_*
Posted 25 February 2012 - 04:49 PM
Oh well, you can lead a horse to water...
Good luck solving your problem, I'm sure someone will come along that has the answer.
#13
Posted 25 February 2012 - 08:59 PM
there is a lot of right left play in the H shaped housing, that movement therefore moves the carriage bolt that the center die is fastened to. With the nuts tight, that is the only way the center die could move, the way it looks to me. BUT, having the center die too high or low would make some extra space that might allow other irregularities to happen. May....be.... I will try this tomorrow, with height matchup as exact as I can get it.
That's the great thing about this forum, enough potters will figure out most things, here's hoping tomorrow produces even walls and straight extrusions.
#14
Posted 27 February 2012 - 06:04 PM
Kiln Repair Tech
L&L Distributor
Owner, Neil Estrick Gallery, LLC
www.neilestrickgallery.com
neil@neilestrickgallery.com
#15
Posted 28 February 2012 - 08:38 AM
What I did last night was shim the sides of the barrel-collar so that the L-R shifting was stopped. I also discovered, that the holes for the cotter pins don't match up exactly from the collar through the barrel and then on through the die holder. I had been checking the die height un assembled and it was a perfect height match. When I put the system together, the center die holder was lifted slightly and then the die outer edge and inner didn't match. Small amount, but I listened to Mark's suggestion.
So what had help a lot was to secure the center die slightly lower than even, so the height mis match was compensated for. Extrusions done with that adjustment and the shims were significantly more even. Tonight I will put it to the big test by running a set of the largest hollow dies.
Much thanks to all suggestions, and Mark, your comments sent me back to examine the height question, that seemed correct, but in use was not.
Happy Potting!
#16
Posted 28 February 2012 - 12:41 PM

Sign In
Register
Help











MultiQuote