I am wanting to do some tri Azial glaze experiments for two reasons One is to further my understanding of glaze ingredients and secondly I want to set them up as a tile display that looks nice and could be used in a class room situation as a study guide of sorts. What books would you recommend or what other sources. Ain't clay fun Kabe
Page 1 of 1
Tri Axial Glaze test where to find information on them
#2
Posted 16 January 2012 - 07:11 AM
Here is a website
http://www.matrix200...axialblends.htm
definition
http://ceramicartsda...triaxial-blend/
It does a thorough job of explaining the process.
here is a slide series
http://coloradoartst...ial-glaze-test/
My tri axial info is on old purple ditto hand outs. A similar system from a book might be the grid system from Ian Curry. Look up Ian's books.
marcia
http://www.matrix200...axialblends.htm
definition
http://ceramicartsda...triaxial-blend/
It does a thorough job of explaining the process.
here is a slide series
http://coloradoartst...ial-glaze-test/
My tri axial info is on old purple ditto hand outs. A similar system from a book might be the grid system from Ian Curry. Look up Ian's books.