How To Get More Even Elec. Firings? full cone diff between shelves?
#1
Posted 03 May 2010 - 10:09 AM
I have a new Scutt 1027 Kilnmaster, hope it is OK to mention brands. I haven't been able to adjust things to get it to have cones even from top to bottom. I am new to firing at home and working my way through this. So far, I have fired with all peeps in and gotton a full cone cooler on the top shelf, with resulting glazes under developed. I put the cones in the same place each time and leave 2" above and below the themocouple with shelves. I use the Corelite shelving.
Next firing I took out the top peep at the suggestion of the Skutt tec guy, got the same looking cones, but that time the bottom was a full cone cooler, like I flipped the temps from top to bottem. Skutt guy said to slow down the last climb, I had set it for 200* per hour to 2195 with a 10 minute hold. He said that was too fast to get even temps through out.
Last night I unloaded a kiln that I has increased the peak soak from 10 minutes to 15 minutes and with a slower, 125* climb to peak, which I set at 22200*. I kept the peeps all in. The cones look more consistent, but I didn't have a top shelf, the only shelf was at mid way, with a full shelf of tall slender pieces with tall handles, so not real dense at the top.
I should add, I don't have a vent, the kiln is outside of my studio in a covered shed. the breeze blows through. The Skutt rep says I won't get even without having peeps out, but when I took them out, nothing improved, only reversed the cool area from top to bottom.
Any advice or similar experiences, I would love to hear. Thanks in advance!
#2
Posted 03 May 2010 - 11:44 AM
The kiln vent helps keep the air circulating inside the kiln which helps keep temps even from top to bottom ...
Having air moving outside really won't help as much.
I soak for twenty minutes then fire down to control the rate of cooling which helps as well.
My top and bottom are still about one half a cone cooler than the center so my firings are aimed at getting the cooler spots to the right temp.
I have also heard of potters adding a blanket of insulation to the lid to help keep the heat in.
Contemporary Fine Colored Porcelain
www.ccpottery.com
"My Artwork would not exist without a thriving global pottery community.
In the isolation of a studio, an artist can begin to feel like an island, but in truth
we are all part of archipelagoes; chains of islands loosely connected by a stream
of information that enhances our Artwork.”
#3
Posted 03 May 2010 - 12:02 PM
If you don't have an undermounted vent, then you should always have at least one peep open. Not for evening out the heat, but for allowing the corrosive gasses to escape. If those gasses are trapped inside, this will shorten the life of your elements.
-Mea
#4
Posted 03 May 2010 - 04:35 PM
h a n s e n
clay lover, on 03 May 2010 - 10:09 AM, said:
I have a new Scutt 1027 Kilnmaster, hope it is OK to mention brands. I haven't been able to adjust things to get it to have cones even from top to bottom. I am new to firing at home and working my way through this. So far, I have fired with all peeps in and gotton a full cone cooler on the top shelf, with resulting glazes under developed. I put the cones in the same place each time and leave 2" above and below the themocouple with shelves. I use the Corelite shelving.
Next firing I took out the top peep at the suggestion of the Skutt tec guy, got the same looking cones, but that time the bottom was a full cone cooler, like I flipped the temps from top to bottem. Skutt guy said to slow down the last climb, I had set it for 200* per hour to 2195 with a 10 minute hold. He said that was too fast to get even temps through out.
Last night I unloaded a kiln that I has increased the peak soak from 10 minutes to 15 minutes and with a slower, 125* climb to peak, which I set at 22200*. I kept the peeps all in. The cones look more consistent, but I didn't have a top shelf, the only shelf was at mid way, with a full shelf of tall slender pieces with tall handles, so not real dense at the top.
I should add, I don't have a vent, the kiln is outside of my studio in a covered shed. the breeze blows through. The Skutt rep says I won't get even without having peeps out, but when I took them out, nothing improved, only reversed the cool area from top to bottom.
Any advice or similar experiences, I would love to hear. Thanks in advance!
Stone House Studio, Alexandria, Virginia
americanpotter.blogspot.com
thesuddenschool.blogspot.com
#5
Posted 03 May 2010 - 08:12 PM
I am doing a controlled down fire, ramp 4 is a drop from 2200 to 1900 and a hold of 30 min at 1900. Then down 125* and hour to 1750, no hold and off. The kiln cooled to 200* to be opened in 13 hours from the 2200 peak.
I didn't have any matt glazes in this firing, so don't know how that will work with these settings.
#7
Posted 04 May 2010 - 08:34 AM
I want to know more about how taking out peeps should help even it up.
#8
Posted 04 May 2010 - 10:16 AM
You really do not want those fumes traveling through your home.
Opening the garage door often just makes it worse as the wind blows in .... Not out!
As to the temp ... I usually go by how full my kiln is and how critical the final temp is.
I confess that I do not use any glazes that are thar fussy so someone else would be a better
judge of that.
Contemporary Fine Colored Porcelain
www.ccpottery.com
"My Artwork would not exist without a thriving global pottery community.
In the isolation of a studio, an artist can begin to feel like an island, but in truth
we are all part of archipelagoes; chains of islands loosely connected by a stream
of information that enhances our Artwork.”
#9
Posted 13 May 2010 - 11:23 AM
#10
Posted 13 May 2010 - 04:15 PM
Chris Campbell, on 04 May 2010 - 10:16 AM, said:
You really do not want those fumes traveling through your home.
Opening the garage door often just makes it worse as the wind blows in .... Not out!
As to the temp ... I usually go by how full my kiln is and how critical the final temp is.
I confess that I do not use any glazes that are thar fussy so someone else would be a better
judge of that.
Stone House Studio, Alexandria, Virginia
americanpotter.blogspot.com
thesuddenschool.blogspot.com
#11
Posted 13 May 2010 - 04:22 PM
h a n s e n
p.s. down draft gas or wood are the most even temp kilns, IMHO
hansen, on 13 May 2010 - 04:15 PM, said:
Chris Campbell, on 04 May 2010 - 10:16 AM, said:
You really do not want those fumes traveling through your home.
Opening the garage door often just makes it worse as the wind blows in .... Not out!
As to the temp ... I usually go by how full my kiln is and how critical the final temp is.
I confess that I do not use any glazes that are thar fussy so someone else would be a better
judge of that.
Stone House Studio, Alexandria, Virginia
americanpotter.blogspot.com
thesuddenschool.blogspot.com
#12
Posted 22 May 2010 - 09:17 AM
hansen, on 13 May 2010 - 04:22 PM, said:
h a n s e n
p.s. down draft gas or wood are the most even temp kilns, IMHO
hansen, on 13 May 2010 - 04:15 PM, said:
Chris Campbell, on 04 May 2010 - 10:16 AM, said:
You really do not want those fumes traveling through your home.
Opening the garage door often just makes it worse as the wind blows in .... Not out!
As to the temp ... I usually go by how full my kiln is and how critical the final temp is.
I confess that I do not use any glazes that are thar fussy so someone else would be a better
judge of that.
#14
Posted 23 May 2010 - 02:20 AM
clay lover, on 22 May 2010 - 09:18 AM, said:
I'm just another potter who has struggled with some of the the same things. So I was looking into the basic textbooks for answers.
"If you are looking at production concerns for wholesale or even production retail you'll want liner glazes with very broad ranges, and for your speciality glazes, again, broader firing ranges. There are about 4-5 ways to make the ranges broader. One glaze I use is called "cone 4-14" for example, so whether it fires to cone 6 or cone 8, you can't tell the difference."
This glaze is called Schwieger's Liner and it is said to be workable from cone 4 to cone 14. I haven't tested this theory, but I looks the same at cone 6 as it does cone 8.
50 Plastic Vitrox
50 gerstley borate
(I substituted Laguna borate)
you can add 10-15% zircopax to make it whiter
This example has a broader firing range because of the use of the element boron.
Lithium as opposed to potassium or sodium gives a broader range, according to the text books.
Zinc oxide will broaden the range.
Magnesium broadens the range.
Use of the mineral feldspar broadens the range.
A combination of minerals which proportionally reflect the ratio called a "eutectic" will lower the melting point and will have the broadest range within a system of similar glazes. However, this really only applies where minerals which are chemically combined are combined in similar ways. In other words, although scientifically we can demonstrate that a frit, which has already been fired and chemically combined, is reground, and if another frit which has been fired the same way and reground the same way, the one closest to the eutectic point will be the both the most fusible and have the lowest melting point.
All this seems kind of abstract, however these are rules of thumb whether you are scratch formulating glazes all the way from Unity to batch, or if you are simply reading recipes online. It is easier to grasp looking at the history of ceramic glaze development. For example, the use of feldspar or porcelain stone was one of the first strides forward into high fire development in China, and an improvement over the mostly wood ash, limestone ash, and clay mixtures which are the basis for earliest glazes. It melts to form a glaze but maintains viscosity through a wider range of temperatures. Wood ash glazes will go from a stable matt glaze to a shiny runny glaze within a fairly narrow window. Hence, feldspar was deemed useful because it was more controlable and predictable.
Zinc glazes were developed in the 19th Century in the USA mostly for oxidation fire in the mid-range. It was added to the basic feldspar, whiting, clay, and flint high fire mixtures mentioned above because it both lowered the melting point but also was more predictable and stable.
Magnesium has it's greatest value when used in reduction high fire studio potter glazes from the '60's and '70's. It can produce a buttery satin matte. In a similar way, it helps get more predicability in the kiln
Eutectic glazes are mostly the concern of the scientist and the laboratory, but back in the day when leaded frits were common, the best ones were generally those in the eutectic. Lead, Silica, and Alumina in different proportions have several different eutectic points at several different cones.
Boron is a strange case because it acts as a refractory at low temperatures, acts as a glass-former, but also has fluxing strength.
So, in applying this to mid-fire electric I would say look for glazes with feldspathic minerals, and/or zinc oxide, and/or boron
does this help?
h a n s e n
Stone House Studio, Alexandria, Virginia
americanpotter.blogspot.com
thesuddenschool.blogspot.com

Sign In
Register
Help











MultiQuote