Recipe
Cobalt Green mat ^6 Oxidation
Neph Syenite was 64.8 increased to 65
Spodumene 13.9
Gerstley Borate 4.6
Ball Clay was 7.4 decreased to 7.2
Whiting 4.6
Silica 4.7
100
bentonite 2
Rutile 2
Cobalt Carbonate 1