- Ceramic Arts Daily - http://ceramicartsdaily.org -

Ferguson’s White Crackle Raku Glaze Recipe

Ferguson’s White Crackle
Raku
Glaze Material
Percentage
Gerstley Borate 65%
Nepheline Syenite 15
Tennessee Ball Clay 5
Tin Oxide 10
silica 5
  100%

 


This recipe is included in 10 Tried and True Raku Glaze Recipes: Recipe Cards for our Favorite Raku Pottery Ceramic Glazes, which is free to Ceramic Arts Daily subscribers.