Matt B Glaze Recipe, Cone 6 Oxidation

Matt “B” Glaze Cone 6 Oxidation
Glaze Material
Percentage
Lithium Carbonate 2.7%
Strontium Carbonate 26.5
Nepheline Syenite 57.5
Kentucky Ball Clay (OM 4) 6.2
Flint 7.1
Total 100.0%
Add:
Bentonite 3.0

 

The matt quality of this glaze is easily affected by colorants, so variations have different surface qualities as well as colors.
For Dark Green Add: For Orange Add:
Copper Carbonate 3% Encapsulated Orange Stain 5%
Nickel Oxide 2% Zirconium Yellow Stain 5%