Frasca Wood Ash Glaze, Cone 6, oxidation or reduction

Frasca Wood Ash Glaze Cone 6, oxidation or reduction
Glaze Material
Whiting 11.36%
Wood Ash (unwashed) 54.56%
Potash Feldspar 11.36%
Ball Clay 11.36%
Silica (Flint) 11.36%
Total: 100.00%
For green, add:
Copper Carbonate 4%
For blue, add:
Cobalt Carbonate 2%