Glaze Material
Gerstley Borate 26%
Nepheline Syenite 48%
Edgar Plastic Kaolin (EPK) 6%
Flint (325 mesh) 20%
Total 100%
Add:
Cobalt Oxide 1%
Light Rutile 4%
Red Iron Oxide 2%