Floating Blue Glaze Recipe
Cone 6 oxidation
Glaze Material
Gerstley Borate 26%
Nepheline Syenite 48%
Edgar Plastic Kaolin (EPK) 6%
Flint (325 mesh) 20%
Total 100%
Add:
Cobalt Oxide 1%
Light Rutile 4%
Red Iron Oxide 2%

This recipe is included in
Top Ten Cone 6 Glaze Recipes: Recipe Cards for Our Favorite Mid-Range Pottery Glazes, which is free to Ceramic Arts Daily subscribers.

Share this post with other ceramic artists:
These icons link to social bookmarking sites where readers can share and discover new web pages.
  • TwitThis
  • Facebook
  • Digg
  • del.icio.us
  • MySpace
  • StumbleUpon
  • Google Bookmarks

1 Comment

  1. LAMIS | August 16th, 2009 at 10:54 pm

    Thank you for the resipi i wish i will have this color on my pot..it’s so beautiful.
    lamis -Australia

You must be logged in to post a comment.