- Ceramic Arts Daily - http://ceramicartsdaily.org -

Blue Green/Copper Red Glaze Recipe, Cone 6 Oxidation or Reduction

Blue Green/Copper Red Glaze Recipe Cone 6
Glaze Material Percentage
Talc 3.30%
Whiting 14.29
Frit 3134 (Ferro) 13.33
Kona F-4 Feldspar 46.16
Edgar Plastic Kaolin 6.40
Flint 16.52
Total 100.00%
Add:
Tin Oxide 2.24%
Zinc Oxide 4.37%
Black Copper Oxide 1.07%

 

This recipe is included in
Top Ten Cone 6 Glaze Recipes: Recipe Cards for Our Favorite Mid-Range Pottery Glazes, which is free to Ceramic Arts Daily subscribers.