Top Crater Glaze Recipe, Cone 08-04 oxidation

Top Crater Glaze Recipe
Cone 08-04 Oxidation
Frit 3134 (Ferro) 52.1%
Edgar Plastic Kaolin (EPK) 11.1
Silica (Flint) 36.8
Total 100%
Add:
Silicon Carbide (100 mesh)  1%

This recipe is included in 10 Tried ad True Low Fire Glaze Recipes: Recipe Cards for our Favorite Low Fire Ceramic Glazes, which is free to Ceramic Arts Daily subscribers.