- Ceramic Arts Daily - http://ceramicartsdaily.org -

Red Green Glaze Recipe, Cone 06 oxidation

Red Green Glaze Recipe
Cone 06 Oxidation
Glaze Material
Percentage
Frit 3134 (Ferro) 50%
Custer Feldspar 50
Total 100%
Add:
Copper Carbonate 3.2%

From Ramon Camarillo, Ceramics Monthly, April 2002.


This recipe is included in 10 Tried and True Low Fire Glaze Recipes: Recipe Cards for our Favorite Low Fire Ceramic Glazes, which is free to Ceramic Arts Daily subscribers.