Matt Glaze Recipe, Cone 06-04 oxidation

Matt Glaze Cone 06-04
 Oxidation
Glaze Material
Percentage
Gerstley Borate 38%
Lithium Carbonate 10
Nepheline Syenite 5
Grolleg Kaolin 5
Flint
42
Total 100%

Add 15% glaze stain for bright pinks and reds; for other bright colors, add 10% glaze stain. Greens require low chrome stains, or bubbling may occur. To get opaque pastels, add 0.5%–2% glaze stain and 8–9.5% Zircopax to total 10%.