Be sure to download your free copy of 10 Tried and True Low Fire Glaze Recipes: Recipe Cards for our Favorite Low Fire Ceramic Glazes, a perfect resource for potters and ceramic artists who are ready to experiment with custom glazes, or for those who have grown tired of their own tried and true glazes.

June 28, 2009

Matt Glaze Recipe, Cone 06-04 oxidation

by Jessica Knapp Read Comments (0)

Matt Glaze
Cone 06-04 Oxidation
Glaze Material
Percentage
Gerstley Borate
38%
Lithium Carbonate
10
Nepheline Syenite
5
Grolleg Kaolin
5
Flint
42




Add 15% glaze stain for bright pinks and reds; for other bright colors, add 10% glaze stain.
Greens require low chrome stains, or bubbling may occur. To get opaque pastels,
add 0.5%–2% glaze stain and 8–9.5% Zircopax to total 10%.

This recipe is included in 10 Tried and True Low Fire Glaze Recipes: Recipe Cards for our Favorite Low Fire Ceramic Glazes, which is free to Ceramic Arts Daily subscribers.

 

Share this post with other ceramic artists:
These icons link to social bookmarking sites where readers can share and discover new web pages.
  • TwitThis
  • Facebook
  • Digg
  • del.icio.us
  • MySpace
  • StumbleUpon
  • Google Bookmarks

You must be logged in to post a comment.