Majolica Glaze
Cone 04 Oxidation
Glaze Material
Percentage
Frit 3124 (Ferro) 65.72%
Kona F-4 Feldspar 17.23
Nepheline Syenite  6.24
Edgar Plastic Kaolin 10.81
Total 100.0%
Add:
Tin Oxide  5.00%
Zircopax 10.00
Bentonite  2.00