- Ceramic Arts Daily - http://ceramicartsdaily.org -

Kari’s Best Transparent Glaze Recipe, Cone 04-02 oxidation

Kari’s Best Transparent Glaze Recipe
Cone 04-02 Oxidation
Glaze Material
Percentage
Gerstley Borate 11.0%
Talc 30.0
Frit 626 (Pemco) 19.0
Frit 3124 (Ferro) 11.0
Spodumene 14.0
EPK Kaolin 15.0
Total 100%
Add:
Wollastonite 5.0%
Veegum T 1.0
CMC Gum
0.4

For Celadon: For Emerald Green:
Copper Carbonate 1.5%  Copper Carbonate 6.0%
For Grape Purple:
 For Blue:
Manganese Dioxide 7.0%  Cobalt Carbonate 1.5%
Copper Carbonate 0.5%  Copper Carbonate 2.0%

From Kari Radasch, Pottery Making Illustrated, May/June 2004.