Kari’s Best Transparent Glaze Recipe
Cone 04-02 Oxidation
Glaze Material
Percentage
Gerstley Borate
11.0%
Talc 30.0
Frit 626 (Pemco) 19.0
Frit 3124 (Ferro) 11.0
Spodumene 14.0
EPK Kaolin 15.0
Total 100%
Add:
Wollastonite
5.0%
Veegum T 1.0
CMC Gum
0.4


For Celadon:
Copper Carbonate 1.5%
For Blue:
Cobalt Carbonate
1.5%
Copper Carbonate 2.0%
For Grape Purple:
Manganese Dioxide
7.0%
Copper Carbonate 0.5%
For Emerald Green:
Copper Carbonate 6.0%

From Kari Radasch, Pottery Making Illustrated, May/June 2004.

This recipe is included in 10 Tried and True Low Fire Glaze Recipes: Recipe Cards for our Favorite Low Fire Ceramic Glazes, which is free to Ceramic Arts Daily subscribers.

 

 

Share this post with other ceramic artists:
These icons link to social bookmarking sites where readers can share and discover new web pages.
  • TwitThis
  • Facebook
  • Digg
  • del.icio.us
  • MySpace
  • StumbleUpon
  • Google Bookmarks

You must be logged in to post a comment.