Hirsh Satin Matt Base Glaze Recipe, Cone 04-02 oxidation

Hirsh Satin Matt Base Glaze Recipe
Cone 04-02 Oxidation
Glaze Material
Gerstley Borate 32%
Lithium Carbonate 9
Whiting 17
Nepheline Syenite 4
EPK Kaolin 4
Silica (Flint) 35
Total 100%



Bentonite 2%


For Green:
Chrome Oxide 1%
For Yellow:
Yellow Stain 8%


For Light Blue
Copper Carbonate 1.5%