Hirsh Satin Matt Base Glaze Recipe
Cone 04-02 Oxidation
Glaze Material
Percentage
Gerstley Borate
32%
Lithium Carbonate 9
Whiting 17
Nepheline Syenite 4
EPK Kaolin 4
Silica (Flint) 35
Total 100%
Add:
Bentonite
2%
For Green:
Chrome Oxide 1%
For Yellow:
Yellow Stain 8%
For Light Blue
Copper Carbonate 1.5%

From Joe Pintz, Ceramics Monthly.

This recipe is included in 10 Tried and True Low Fire Glaze Recipes: Recipe Cards for our Favorite Low Fire Ceramic Glazes, which is free to Ceramic Arts Daily subscribers.
Share this post with other ceramic artists:
These icons link to social bookmarking sites where readers can share and discover new web pages.
  • TwitThis
  • Facebook
  • Digg
  • del.icio.us
  • MySpace
  • StumbleUpon
  • Google Bookmarks

1 Comment

  1. Jennifer | September 20th, 2009 at 3:32 am

    Has anyone found a good GB substitute to use with this glaze recipe?

    Thanks

You must be logged in to post a comment.