- Ceramic Arts Daily - http://ceramicartsdaily.org -

Crater Underglaze Recipe, Cone 08-04 oxidation

Crater Underglaze Recipe
Cone 08-04 Oxidation
Glaze Material
Percentage
Borax (powder) 5%
Talc 15
Frit 3269 25
EPK 15
Kentucky Ball Clay (OM4) 15
Silica (Flint) 25
Total 100%
Add:
Silicon Carbide (100 mesh)  2%


This recipe is included in 10 Tried and True Low Fire Glaze Recipes: Recipe Cards for our Favorite Low Fire Ceramic Glazes, which is free to Ceramic Arts Daily subscribers.