Leaving Bariumville: Replacing Barium Carbonate in Cone 10 Glazes

by Daniel Semler Read Comments (2)

The author tested and demonstrated barium carbonate substitutions for the following glazes:

Blue Matt, Celadon, Iron-Rutile Matt, Translucent Blue, Opaque Gray-Tan Matt

Also, check out the author’s explanation of Molar Versus Weight Substitution, as well as his Conclusions.

Barium carbonate has long been used as an ingredient in high-fire glazes, sometimes conferring unique properties upon glazes. One of the alkaline earth carbonates, it has also been used as rat poison (large doses can be toxic to humans as well). Glazes containing it ought to be checked for barium leaching if they are intended to hold food or drink, or reserved for surfaces that do not come into contact with food. It is not my intent to present the research on barium toxicity here, but to present a course of action for replacing it in glazes.

Largely as a result of its toxicity, questions arise, from time to time, as to what might best be substituted for barium carbonate, and how much should be used. Hot on the heels of such questions are those about how similar the glaze will be to the original. I had come across some such discussions on the Clayart listserv and wondered just how successful one could be in replacing barium carbonate in a glaze.

The usual replacement is strontium carbonate. Whiting is another candidate, because it is also an alkaline earth. The final alkaline earth choice is magnesium carbonate but it produces a more viscous melt and, in large quantities, promotes crawling. In this test series, I worked with strontium carbonate and whiting as substitutes.

I began by acquiring an old secondhand copy of James Chappell’s The Potter’s Complete Book of Clay and Glazes, as well as various other recipe sources. I then went through them and gathered all the barium containing Cone 10 glazes for which I already had, or could easily get, the materials. This gave me 34 glazes ranging from matt to satin to gloss, with a variety of colorants and varying amounts of barium carbonate.

The study consisted of mixing each one of these glazes in three forms, and then comparing the fired results. The first was the original, the second used strontium carbonate in place of the barium carbonate, and the third used whiting. All tests were done on Glacia Cone 10 porcelain from Clay Planet in Santa Clara, California. I mixed up each glaze and applied it to two tests pieces each, one for an oxidation firing, the other for reduction.

All substitutions were performed with glaze-calculation software. Substitutions were made on a molar basis so the ratios of total fluxes to alumina and silica were maintained (see “Molar Versus Weight Substitution” on page 44). In doing this, one finds that only 75% as much strontium carbonate, by weight, is required, and only 51% as much whiting.

All tests were fired in a downdraft gas kiln at the Foster City recreation center, where I have made pottery for a number of years. Needless to say, I am very grateful to the kiln loaders and to Tammy Burwell who fired these pieces.


This article was originally published in Ceramics Monthly.
To get great content like this delivered right to your door, subscribe today!


After firing all the tests, I finally had lots of information. The time had come to try to make sense of it! In order to establish some criteria for matching, I looked at the fired samples a number of times and made notes on each sample on its own and in comparison with the original barium containing glaze. In the end, I settled on five properties that are significant in comparing the glazes. These are gloss, color, fit, stiffness and feel. In general the stiffness, or degree to which the glaze moved, was the easiest property to duplicate in the substitution. Surface feel was the hardest, driven largely by the difference in feel between barium and strontium matts, the strontium being drier. There were a number of examples among the whiting substitutes that showed a greater tendency to run.

Finally, there is a set of glazes for which the whiting substitute produced a significantly, though not drastically, runnier glaze, than either the original or the strontium variant. This happens when the glaze is a matt or satin and the original glaze contains substantial quantities of barium carbonate and whiting to begin with.

The Tests

Blue Matt

The poster-child for

The poster-child for the difficulty in replacing barium carbonate in a glaze is SG-259, a silky matt barium copper blue. SG-259 is a fabulous glaze that is a completely different color when strontium carbonate (on the right) is used. The surface feel is very similar, perhaps a little smoother in the strontium glaze.

Left: SG-259 Opaque Blue Matt
with Barium
(Cone 10)

Barium Carbonate
38.4
Nepheline Syenite
48.0
Tennessee Ball Clay #10
6.1
Silica 7.5
Total
100.0
Add:

Copper Carbonate
 4.0
Bentonite 1.0

Right: SG-259 Opaque Blue Matt
with Strontium
(Cone 10)

Strontium Carbonate
31.9
Nepheline Syenite
53.1
Tennessee Ball Clay #10
6.7
Silica 8.3
Total
100.0
Add:

Copper Carbonate
4.0
Bentonite 1.0

 

Celadon

Celadons tended to show very slight color variation with the fluxes. Racer Celadon 3, for example, is slightly greener in the strontium case.

Celadons tended to show very slight color variation with the fluxes. Racer Celadon 3, for example, is slightly greener in the strontium case.

Left: Racer Celadon 3
with Barium
(Cone 10)
Barium Carbonate
6.62
Talc
3.53
Whiting
11.03
Custer Feldspar
22.05
F-4 Feldspar
21.93
Bentonite 2.21
Silica 32.63
Total 100.00
Add:
Chrome 0.05
Yellow Iron 1.10
Barium Unity Formula
BaO *0.13
CaO *0.48
MgO *0.11
K2O *0.14
Na2O *0.14
Al2O3 0.33
SiO2  4.29
Middle: Racer Celadon 3
with Strontium
(Cone 10)
Strontium Carbonate
5.0
Talc
3.6
Whiting
11.2
Custer Feldspar
22.4
F-4 Feldspar
22.3
Bentonite 2.2
Silica 33.3
Total 100.0
Add:
Chrome 0.1
Yellow Iron 1.1
Strontium Unity Formula
SrO *0.13
CaO *0.48
MgO *0.11
K2O *0.14
Na2O *0.14
Al2O3 0.33
SiO2  4.30
Right: Racer Celadon 3
with Whiting
(Cone 10)
Talc
3.6
Whiting 14.9
Custer Feldspar
22.8
F-4 Feldspar
22.7
Bentonite 2.3
Silica 33.7
Total 100.0
Add:
Chrome 0.1
Yellow Iron 1.1
Calcium Unity Formula
 
CaO *0.61
MgO *0.11
K2O *0.14
Na2O *0.14
Al2O3 0.33
SiO2  4.30

 

Molar Versus Weight Substitution

Let’s consider two methods of material substitution in glazes. The first is by raw material weight and the second is molar (molecular) substitution. Substitution by weight is exactly what it sounds like; replace 25 grams of barium carbonate in a recipe with 25 grams of whiting. While this will produce a glaze that can be fired, it’s likely that it will be runnier than the original. The reason is that 25 grams of whiting supplies far more molecules of flux than 25 grams of barium carbonate does. Substitution on a molar basis, on the other hand, will give a more comparable glaze. In this case, the total number of molecules of flux will remain the same relative to the alumina and silica. This is significant because glazes are formed by chemical reactions between the molecules during the firing.

The original recipe above contains 6.62% barium carbonate by weight, but the strontium version only has 5% strontium carbonate, and the calcium version only has 3.7% whiting by weight. Now look at the unity formulae; the portion of the fluxes that is substituted remains a steady 0.13. Thus, the number of molecules of each component in the fired glaze is more important than how much the raw materials weigh. Molar substitution does not guarantee that the glaze will be the same as the original, but the general degree of melting will be about the same in most cases. There are glaze books that explain how to calculate this process longhand, but molar substitution is readily accomplished with modern glaze software.

 

Iron-Rutile Matt

In SG-266 we have an iron and rutile matt glaze. Here the match is in between. The color is not quite the same, and the surface texture is slightly off, the strontium being perhaps very slightly drier, though this could be application thickness as it's clearly important with this glaze. Some darker crystallization is noticeable in the whiting version. Strontium would appear to be the better substitute here, but more testing would be required to know for sure.

In SG-266 we have an iron and rutile matt glaze. Here the match is in between. The color is not quite the same, and the surface texture is slightly off, the strontium being perhaps very slightly drier, though this could be application thickness as it's clearly important with this glaze. Some darker crystallization is noticeable in the whiting version. Strontium would appear to be the better substitute here, but more testing would be required to know for sure.

Left: SG-266 Opaque Cordova-Brown with Barium
(Cone 10)

Barium Carbonate
23.6
Whiting
9.5
Custer Feldspar
56.0
Tennessee Ball Clay #10
10.9
Total 100.0
Add:
Ultrox 8.8
Red Iron Oxide 4.5
Rutile 2.2
Bentonite 1.0

Middle: SG-266 Opaque Cordova-Brown with Strontium
(Cone 10)

Strontium Carbonate
18.8
Whiting
10.1
Custer Feldspar
59.6
Tennessee Ball Clay #10
11.6
Total 100.0
Add:
Ultrox 8.8
Red Iron Oxide 4.5
Rutile 2.2
Bentonite 1.0

Right: SG-266 Opaque Cordova-Brown with Whiting
(Cone 10)

 

Whiting
24.3
Custer Feldspar
63.4
Tennessee Ball Clay #10
12.3
Total 100.0
Add:
Ultrox 8.8
Red Iron Oxide 4.5
Rutile 2.2
Bentonite 1.0

 

Translucent Blue

By way of contrast, SG-262 shows just how good a substitute strontium carbonate or whiting can be. SG-262 contains both copper carbonate and cobalt oxide and gives a very deep blue gloss, though it's billed as a translucent turquoise blue matt. It can readily be seen that substitution here is extremely good. The amount of movement is similar, the gloss is maintained, the color is unperturbed. This test showed that it was easier to substitute in gloss glazes.

By way of contrast, SG-262 shows just how good a substitute strontium carbonate or whiting can be. SG-262 contains both copper carbonate and cobalt oxide and gives a very deep blue gloss, though it's billed as a translucent turquoise blue matt. It can readily be seen that substitution here is extremely good. The amount of movement is similar, the gloss is maintained, the color is unperturbed. This test showed that it was easier to substitute in gloss glazes.

Left: SG-262 Translucent
Turquoise-Blue Matt with Barium
(Cone 10)

Barium Carbonate
7.2
Cornwall Stone
34.0
Dolomite
6.9
Whiting
14.8
Custer Feldspar
33.2
EPK Kaolin
3.9
Total  100.0
Add:
Cobalt Oxide
1.0
Copper Carbonate 2.0

Middle: SG-262 Translucent
Turquoise-Blue Matt with Strontium
(Cone 10)

Strontium Carbonate
5.5
Cornwall Stone
34.6
Dolomite
7.0
Whiting
15.1
Custer Feldspar
33.8
EPK Kaolin
4.0
Total  100.0
Add:
Cobalt Oxide
1.0
Copper Carbonate
2.0

Right: SG-262 Translucent
Turquoise-Blue Matt with Whiting
(Cone 10)

 

Cornwall Stone
35.2
Dolomite
7.2
Whiting
19.2
Custer Feldspar
34.4
EPK Kaolin
4.0
Total  100.0
Add:
Cobalt Oxide
1.0
Copper Carbonate
2.0

 

Opaque Gray-Tan Matt

SG-302 contains nearly 10% rutile and is a satin matt glaze. This test was very interesting because the buttery barium matt feel is entirely gone in the strontium glaze, which is very dry. The color match is not good where thin, and the speckling in the barium glaze where it's thickest is not repeated in the strontium glaze. The whiting version is orange rather than yellow. This and SG-266 would suggest that iron and rutile in large quantities in nonglossy glazes may be difficult to get exactly right. It is interesting to note that some SrO matts may be drier than BaO matts with the same molar concentration of flux, and that there may be some pitting in such glazes.

SG-302 contains nearly 10% rutile and is a satin matt glaze. This test was very interesting because the buttery barium matt feel is entirely gone in the strontium glaze, which is very dry. The color match is not good where thin, and the speckling in the barium glaze where it's thickest is not repeated in the strontium glaze. The whiting version is orange rather than yellow. This and SG-266 would suggest that iron and rutile in large quantities in nonglossy glazes may be difficult to get exactly right. It is interesting to note that some SrO matts may be drier than BaO matts with the same molar concentration of flux, and that there may be some pitting in such glazes.

Left: SG-302 Opaque Gray-Tan Matt with Barium
(Cone 10)

Barium Carbonate
23.26
Whiting
9.80
Custer Feldspar
55.96
Ball Clay (OM#4)
10.98
Total
100.00
Rutile 9.20
Ultrox 7.70
Bentonite 1.20

Middle: SG-302 Opaque Gray-Tan Matt with Strontium
(Cone 10)

Strontium Carbonate
18.52
Whiting
10.40
Custer Feldspar
59.42
Ball Clay (OM#4)
11.66
Total
100.00
Rutile 9.20
Ultrox 7.70
Bentonite 1.20

Right: SG-302 Opaque Gray-Tan Matt with Whiting
(Cone 10)

 

Whiting
24.3
Custer Feldspar
62.4
Ball Clay (OM#4)
12.2
Total
100.00
Rutile 10.3
Ultrox 7.7
Bentonite 1.2

 

Conclusions

These tests suggest the following, admittedly tentative, conclusions, though there are bound to be exceptions:

1. Less than about 0.2 molar equivalents of barium oxide appears to be readily substitutable.

2. Gloss glazes are easier to reproduce by substituting other alkaline earth carbonates for barium carbonate than matt glazes, even with relatively high concentrations of flux.

3. In matts where the matting is primarily driven by the flux, substitution is perhaps the least successful.

4. Glazes containing certain colorants are difficult to substitute with higher concentrations of flux, the classic being barium matt copper blue. Iron also can change color when barium is substituted.

5. The success of these substitutions was little affected by reduction versus oxidation atmospheres.

As always, this testing raises many questions. However, it does show that calcium and/or strontium are excellent, safe substitutes for barium in many glazes. Strontium does produce dryer matts and less dramatic copper blues. Calcium can make a glaze runnier, depending on the recipes. This knowledge should help artists looking for safer glaze ingredients for use in their studios.

the author When he is not making an insane number of test tiles, Daniel Semler develops software and makes pots in Belmont, California. For further information, see www.clayosmos.com.

Tags: , , , , , , , ,

Share this post with other ceramic artists:
These icons link to social bookmarking sites where readers can share and discover new web pages.
  • TwitThis
  • Facebook
  • Digg
  • del.icio.us
  • MySpace
  • StumbleUpon
  • Google Bookmarks

2 Comments

  1. Cheri | December 6th, 2009 at 5:53 pm

    sutbtituting strontium for barium means it is still toxic and not food safe, and not as beautiful!

  2. Sherman | December 8th, 2009 at 11:19 am

    Cheri, are you sure you’re not confusing strontium carbonate with other strontium compounds (like strontium 89/90, which are associated with nuclear reactions)? Various sources, including material safety data sheets for strontium carbonate, indicate that it has a toxicity rating of 1, which is slight. The only appreciable risk listed is associated with ingestion of large amounts of the material, but even then the risk is due to the CO2 it releases, not the strontium. I hope this helps.

You must be logged in to post a comment.